e01.org

The Dyeing of Cotton Fabrics: A Practical Handbook for the Dyer and Student

687,322 chars · English

The Project Gutenberg eBook of The Dyeing of Cotton Fabrics: A Practical Handbook for the Dyer and Student

This eBook is for the use of anyone anywhere in the United States and
most other parts of the world at no cost and with almost no restrictions
whatsoever. You may copy it, give it away or re-use it under the terms
of the Project Gutenberg License included with this eBook or online
at www.gutenberg.org. If you are not located in the United States,
you will have to check the laws of the country where you are located
before using this eBook.

Title: The Dyeing of Cotton Fabrics: A Practical Handbook for the Dyer and Student

Author: Franklin Beech

Release date: April 27, 2007 [eBook #21224]
Most recently updated: January 2, 2021

Language: English

Other information and formats: www.gutenberg.org/ebooks/21224

Credits: Produced by Audrey Longhurst, Labyrinths and the Online
Distributed Proofreading Team at https://www.pgdp.net

*** START OF THE PROJECT GUTENBERG EBOOK THE DYEING OF COTTON FABRICS: A PRACTICAL HANDBOOK FOR THE DYER AND STUDENT ***

Produced by Audrey Longhurst, Labyrinths and the Online
Distributed Proofreading Team at https://www.pgdp.net

THE

DYEING OF COTTON FABRICS

_A PRACTICAL HANDBOOK FOR THE DYER AND STUDENT_

BY

FRANKLIN BEECH

PRACTICAL COLOURIST AND CHEMIST

_ILLUSTRATED BY FORTY-FOUR ENGRAVINGS_

LONDON SCOTT, GREENWOOD & CO. 19 LUDGATE HILL, E.C.

1901

[_All rights reserved_]

PREFACE.

In writing this little book the author believes he is supplying a want
which most Students and Dyers of Cotton Fabrics have felt--that of a
small handbook clearly describing the various processes and operations
of the great industry of dyeing Cotton.

The aim has not been to produce a very elaborate treatise but rather a
book of a convenient size, and in order to do so it has been necessary
to be brief and to omit many matters that would rightfully find a place
in a larger treatise, but the author hopes that nothing of importance
has been omitted. The most modern processes have been described in some
detail; care has been taken to select those which experience shows to be
thoroughly reliable and to give good results.

FRANKLIN BEECH.

_May, 1901._

CONTENTS.

CHAPTER I.
PAGE
STRUCTURE AND CHEMISTRY OF THE COTTON FIBRE 1
Action of Alkalies 6
Action of Acids on Cellulose 9
Action of Sulphuric Acid on Cotton 10
Action of Hydrochloric Acid 11
Action of Nitric Acid 12
Action of Oxidising Agents on Cellulose or Cotton 16

CHAPTER II.

SCOURING AND BLEACHING OF COTTON 23
Stains and Damages in Bleached Goods 50

CHAPTER III.

DYEING MACHINERY AND DYEING MANIPULATIONS 53
Hand Dyeing 53
Dyeing Machines 57
Dyeing, Slubbing, Sliver or Carded Cotton and Wool 58
Cop Dyeing 64

CHAPTER IV.

THE PRINCIPLES AND PRACTICE OF COTTON DYEING 82
(1) Direct Dyeing 85
(2) Direct Dyeing followed by Fixation with Metallic Salts 112
(3) Direct Dyeing followed by Fixation with Developers 128
(4) Direct Dyeing followed by Fixation with Couplers 139
(5) Dyeing on Tannic Mordant 147
(6) Dyeing on Metallic Mordants 156
(7) Production of Colour Direct upon Cotton Fibres 181
(8) Dyeing Cotton by Impregnation with Dye-stuff Solution 198

CHAPTER V.

DYEING UNION (MIXED COTTON AND WOOL) FABRICS 208

CHAPTER VI.

DYEING HALF SILK (COTTON-SILK, SATIN) FABRICS 225
Method of Dyeing 225

CHAPTER VII.

OPERATIONS FOLLOWING DYEING 239
Washing, Soaping, Drying 239

CHAPTER VIII.

TESTING OF THE COLOUR OF DYED FABRICS 257

CHAPTER IX.

EXPERIMENTAL DYEING AND COMPARATIVE DYE TESTING 262

LIST OF ILLUSTRATIONS

FIG. PAGE
1. Cotton Fibre 5
1A. Cross-section of Cotton Fibre 5
2. Mercerised Cotton Fibre 7
2A. Cross-section of Mercerised Cotton Fibre 7
3. Silkified Cotton Fibre 9
3A. Cross-section of Silkified Cotton Fibre 9
4. Mather & Platt's Low-pressure Bleaching Kier 31
5. Mather & Platt's Yarn-bleaching Kier 49
6. Rectangular Dye-tank 54
7. Round Dye-tub 54
8. Section of Dye-vat 56
9. Delahunty's Dyeing Machine 58
10. Obermaier Dyeing Machine 59
11. Holliday's Yarn-dyeing Machine 60
12. Klauder-Weldon Dyeing Machine 62
13. Graemiger Cop-dyeing Machine 65
14. Graemiger Cop-dyeing Machine 66
15. Beaumont's Cop-dyeing Machine 67
16. Warp-dyeing Machine 70
17. Warp-dyeing Machine 71
18. Dye-jiggers 72
19. Dye-jigger 73
20. Jig Wince 75
21. Cloth-dyeing Machine 76
22. Dye Beck 77
23. Holliday's Machine for Hawking Cloth 78
24. Continuous Dyeing Machine 79
25. Padding Machine 80
26. Padding Machine 81
27. Dye-tub for Paranitroaniline Red 191
28. Padding Machine for Paranitroaniline Red 192
29. Developing Machine for Paranitroaniline Red 194
30. Indigo Dye-vat for Cloth 199
31. Squeezing Rollers 240
32. Yarn-washing Machine 243
33. Dye-house Washing Machine 244
34. Cloth-washing Machine 245
35. Cloth-washing Machine 247
36. Washing and Soaping Vats 248
37. Steaming Cottage 249
38. Steaming and Ageing Chamber 250
39. Hydro-extractor 251
40. Hydro-extractor 252
41. Automatic Yarn-dryer 253
42. Truck Yarn-dryer 254
43. Drying Cylinders 255
44. Experimental Dye-bath 263

CHAPTER I.

STRUCTURE AND CHEMISTRY OF THE COTTON FIBRE.

There is scarcely any subject of so much importance to the bleacher,
textile colourist or textile manufacturer as the structure and chemistry
of the cotton fibre with which he has to deal. By the term chemistry we
mean not only the composition of the fibre substance itself, but also
the reactions it is capable of undergoing when brought into contact with
various chemical substances--acids, alkalies, salts, etc. These
reactions have a very important bearing on the operations of bleaching
and dyeing of cotton fabrics.

A few words on vegetable textile fibres in general may be of interest.
Fibres are met with in connection with plants in three ways.

First, as cuticle or ciliary fibres or hairs; these are of no practical
use, being much too short for preparing textile fabrics from, but they
play an important part in the physiology of the plant.

Second, as seed hairs; that is fibres that are attached to the seeds of
many plants, such, for instance, as the common thistle and dandelion;
the cotton fibre belongs to this group of seed hairs, while there are
others, kapok, etc., that have been tried from time to time in spinning
and weaving, but without much success. These seed hairs vary much in
length, from 1/4 inch to 1-1/2 inches or even 2 inches; each fibre
consists of a single unit. Whether it is serviceable as a textile fibre
depends upon its structure, which differs in different plants, and also
upon the quantity available.

The third class of fibre, which is by far the most numerous, consists of
those found lying between the bark or outer cuticle and the true woody
tissues of the plant. This portion is known as the bast, and hence these
fibres are known as "bast fibres". They are noticeable on account of the
great length of the fibres, in some cases upwards of 6 feet, which can
be obtained; but it should be pointed out that these long fibres are not
the unit fibres, but are really bundles of the ultimate fibres
aggregated together to form one long fibre, as found in and obtained
from the plant. Thus the ultimate fibres of jute are really very
short--from 1/10 to 1/8 of an inch in length; those of flax are somewhat
longer. Jute, flax, China grass and hemp are common fibres which are
derived from the bast of the plants.

There is an important point of difference between seed fibres and bast
fibres, that is in the degree of purity. While the seed fibres are
fairly free from impurities--cotton rarely containing more than 5 per
cent.--the bast fibres contain a large proportion of impurity, from 25
to 30 per cent. as they are first obtained from the plant, and this
large quantity has much influence on the extent and character of the
treatments to which they are subjected.

As regards the structure of the fibres, it will be sufficient to say
that while seed hairs are cylindrical and tubular and have thin walls,
bast fibres are more or less polygonal in form and are not essentially
tubular, having thick walls and small central canals.

=The Cotton Fibre.=--The seed hairs of the cotton plant are separated
from the seeds by the process of ginning, and they then pass into
commerce as raw cotton. In this condition the fibre is found to consist
of the actual fibrous substance itself, containing, however, about 8 per
cent. of hygroscopic or natural moisture, and 5 per cent. of impurities
of various kinds, which vary in amount and in kind in various
descriptions of cotton. In the process of manufacture into cotton
cloths, and as the material passes through the operations of bleaching,
dyeing or printing, the impurities are eliminated.

=Impurities of the Cotton Fibre.=--Dr. E. Schunck made an investigation
many years ago into the character of the impurities, and found them to
consist of the following substances:--

=Cotton Wax.=--This substance bears a close resemblance to carnauba wax.
It is lighter than water, has a waxy lustre, is somewhat translucent, is
easily powdered, and melts below the boiling point of water. It is
insoluble in water, but dissolves in alcohol and in ether. When boiled
with weak caustic soda it melts but is not dissolved by the alkali; it
can, however, be dissolved by boiling with alcoholic caustic potash.
This wax is found fairly uniformly distributed over the surface of the
cotton fibre, and it is due to this fact that raw cotton is wetted by
water only with difficulty.

=Fatty Acids.=--A solid, fatty acid, melting at 55° C. is also present
in cotton. Probably stearic acid is the main constituent of this fatty
acid.

=Colouring Matter.=--Two brown colouring matters, both containing
nitrogen, can be obtained from raw cotton. One of these is readily
soluble in alcohol, the other only sparingly so. The presence in
relatively large quantities of these bodies accounts for the brown
colour of Egyptian and some other dark-coloured varieties of cotton.

=Pectic Acid.=--This is the chief impurity found in raw cotton. It can
be obtained in the form of an amorphous substance of a light yellow
colour, not unlike gum in appearance. It is soluble in boiling water,
and the solution has a faint acid reaction. Acids and many metallic
salts, such as mercury, chloride and lead acetate, precipitate pectic
acid from its solutions. Alkalies combine with it, and these compounds
form brown substances, are but sparingly soluble in water, and many of
them can be precipitated out by addition of neutral salts, like sodium
and ammonium chlorides.

=Albumens.=--A small quantity of albuminous matter is found among the
impurities of cotton.

=Structure of the Cotton Fibre.=--The cotton fibre varies in length from
1 to 2 inches, not only in fibres of the same class but also in fibres
from different localities--Indian fibres varying from 0.8 in the
shortest to 1.4 in the longest stapled varieties; Egyptian cotton fibres
range from 1.1 to 1.6 inches long; American cotton ranges from 0.8 in
the shortest to 2 inches in the longest fibres. The diameter is about
1/1260 of an inch. When seen under the microscope fully ripe cotton
presents the appearance of irregularly twisted ribbons, with thick
rounded edges. The thickest part is the root end, or point of attachment
to the seed. The free end terminates in a point. The diameter is fairly
uniform through 3/4 to 7/8 of its length, the rest is taper. In Fig. 1
is given some illustrations of the cotton fibre, showing this twisted
and ribbon-like structure, while in Fig. 1A is given some transverse
sections of the fibre. These show that it is a collapsed cylinder, the
walls being of considerable thickness when compared with the internal
bore or canal.

Perfectly developed, well-formed cotton fibres always present this
appearance. But all commercial cottons contain more or less of fibres
which are not perfectly developed or are unripe. These are known as
"dead fibres"; they do not spin well and they do not dye well. On
examination under the microscope it is seen that these fibres have not
the flattened, twisted appearance of the ripe fibres, but are flatter,
and the central canal is almost obliterated and the fibres are but
little twisted. Dead fibres are thin, brittle and weak.

=Composition of the Cotton Fibres.=--Of all the vegetable textile fibres
cotton is found to have the simplest chemical composition and to be, as
it were, the type substance of all such fibres, the others differing
from it in several respects. When stripped of the comparatively small
quantities of impurities, cotton is found to consist of a substance to
which the name of cellulose has been given.

[Illustration: FIG. 1.--Cotton Fibre.]
[Illustration: FIG. 1A.]

Cellulose is a compound of the three elements, carbon, hydrogen and
oxygen, in the proportions shown in the following analysis:--

Carbon, 44.2 per cent.,
Hydrogen, 6.3 per cent.,
Oxygen, 49.5 per cent.,

which corresponds to the empirical formula C{6}H{10}O{5}, which shows
it to belong to the group of carbo-hydrates, that is, bodies which
contain the hydrogen and oxygen present in them in the proportion in
which they are present in water, namely H{2}O.

Cellulose may be obtained in a pure condition from cotton by treatment
with alkalies, followed by washing, and by treatment with alkaline
hypochlorites, acids, washing and, finally, drying. As thus obtained it
is a white substance having the form of the fibre from which it is
procured, showing a slight lustre, and is slightly translucent. The
specific gravity is 1.5, it being heavier than water. It is
characterised by being very inert, a property of considerable value from
a technical point of view, as enabling the fibres to stand the various
operations of bleaching, dyeing, printing, finishing, etc. Nevertheless,
by suitable means, cellulose can be made to undergo various chemical
decompositions which will be noted in some detail.

Cellulose on exposure to the air will absorb moisture or water. This is
known as hygroscopic moisture, or "water of condition". The amount in
cotton is about 8 per cent., and it has a very important bearing on the
spinning properties of the fibre, as it makes the fibre soft and
elastic, while absolutely dry cotton fibre is stiff, brittle and
non-elastic; hence it is easier to spin and weave cotton in moist
climates or weather than in dry climates or weather. Cotton cellulose is
insoluble in all ordinary solvents, such as water, ether, alcohol,
chloroform, benzene, etc., and these agents have no influence in any way
on the material, but it is soluble in some special solvents that will be
noted later on.

ACTION OF ALKALIES.

The action of alkalies on cellulose or cotton is one of great importance
in view of the universal use of alkaline liquors made from soda or
caustic soda in the scouring, bleaching and dyeing of cotton, while
great interest attaches to the use of caustic soda in the "mercerising"
of cotton.

Dilute solutions of the caustic alkalies, caustic soda or caustic
potash, of from 2 to 7 per cent. strength, have no action on cellulose
or cotton, in the cold, even when a prolonged digestion of the fibre
with the alkaline solution takes place. Caustic alkali solutions of from
1 to 2 per cent. strength have little or no action even when used at
high temperatures and under considerable pressure--a fact of very great
importance from a bleacher's point of view, as it enables him to subject
cotton to a boil in kiers, with such alkaline solutions at high
pressures, for the purpose of scouring the cotton, without damaging the
fibre itself.

[Illustration: FIG. 2.--Mercerised Cotton Fibre.]
[Illustration: FIG. 2A.]

Solutions of caustic soda of greater strength than 3 per cent. tend,
when boiled under pressure, to convert the cellulose into soluble
bodies, and as much as 20 per cent. of the fibre may become dissolved
under such treatment. The action of strong solutions of caustic soda or
caustic potash upon cellulose or cotton is somewhat different. Mercer
found that solutions containing 10 per cent. of alkali had a very
considerable effect upon the fibre, causing it to swell up and become
gelatinous and transparent in its structure, each individual cotton
fibre losing its ribbon-like appearance, and assuming a rod-like form,
the central canal being more or less obliterated. This is shown in Fig.
2 and 2A, where the fibre is shown as a rod and the cross section in
Fig. 2A has no central canal. The action which takes place is as
follows: The cellulose enters into a combination with the alkali and
there is formed a sodium cellulose, which has the formula
C{6}H{10}O{5}2NaOH. This alkali cellulose, however, is not a stable
body; by washing with water the alkali is removed, and hydrated
cellulose is obtained, which has the formula C{6}H{10}O{5}H{2}O.
Water removes the whole of the alkali, but alcohol only removes one
half. It has been observed that during the process of washing with water
the fibre shrinks very much. This shrinkage is more particularly to be
observed in the case of cotton. As John Mercer was the first to point
out the action of the alkaline solutions on cotton, the process has
become known as "mercerisation".

Solutions of caustic soda of 1.000 or 20° Tw. in strength have very
little mercerising action, and it is only by prolonged treatment that
mercerisation can be effected. It is interesting to observe that the
addition of zinc oxide to the caustic solution increases its mercerising
powers. Solutions of 1.225 to 1.275 (that is from 45° to 55° Tw. in
strength) effect the mercerisation almost immediately in the cold, and
this is the best strength at which to use caustic soda solutions for
this purpose. In addition to the change brought about by the shrinking
and thickening of the material, the mercerised fibres are stronger than
the untreated fibres, and at the same time they have a stronger affinity
for dyes, a piece of cloth mercerised taking up three times as much
colouring matter as a piece of unmercerised cloth from the same
dye-bath.

The shrinkage of the cotton, which takes place during the operation of
washing with water, was for a long time a bar to any practical
application of the "mercerising" process, but some years ago Lowe
ascertained that by conducting the operation while the cotton was
stretched or in a state of tension this shrinkage did not take place;
further, Thomas and Prevost found that the cotton so treated gained a
silky lustre, and it has since been ascertained that this lustre is
most highly developed with the long-stapled Egyptian and Sea Island
cottons. This mercerising under tension is now applied on a large scale
to produce silkified cotton. When viewed under the microscope, the
silkified cotton fibres have the appearance shown in Fig. 3, long
rod-like fibres nearly if not quite cylindrical; the cross section of
those fibres has the appearance shown in Fig. 3A. This structure fully
accounts for the silky lustre possessed by the mercerised fibres. Silky
mercerised cotton has very considerable affinity for dye-stuffs, taking
them up much more readily from dye-baths, and it is dyed in very
brilliant shades.

[Illustration: FIG. 3.--Silkified Cotton Fibre.]

[Illustration: FIG 3A.]

In the chapter on Scouring and Bleaching of Cotton, some reference will
be made to the action of alkalies on cotton.

ACTION OF ACIDS ON CELLULOSE.

The action of acids on cellulose is a very varied one, being dependent
upon several factors, such as the particular acid used, the strength of
the acid, duration of action, temperature, etc. As a rule, organic
acids--for example acetic, oxalic, citric, tartaric--have no action on
cellulose or cotton. Solutions of sulphuric acid or hydrochloric acid of
2 per cent. strength have practically no action in the cold, and if
after immersion the cotton or cellulose be well washed there is no
change of any kind. This is important, as in certain operations of
bleaching cotton and other vegetable fibres it is necessary to sour
them, which could not be done if acids acted on them, but it is
important to thoroughly wash the goods afterwards. When the acid
solutions are used at the boil they have a disintegrating effect on the
cellulose, the latter being converted into hydrocellulose. When dried,
the cellulose is very brittle and powdery, which in the case of cotton
yarn being so treated would show itself by the yarn becoming tender and
rotten. The degree of action varies with the temperature (the higher
this is the stronger the action), and also according to the strength of
the acid solution. Thus a 10 per cent. solution of sulphuric acid used
at a temperature of 80° C. begins to act on cotton after about five
minutes' immersion, in half an hour there is a perceptible amount of
disintegration, but the complete conversion of the cotton into
hydrocellulose requires one hour's immersion. A dilute acid with 8
volumes of water, used in the cold, takes three hours' immersion before
any action on the cotton becomes evident.

ACTION OF SULPHURIC ACID ON COTTON.

When cellulose (cotton) is immersed in strong sulphuric acid the cotton
becomes gradually dissolved; as the action progresses cellulose
sulphates are formed, and some hydrolytic action takes place, with the
formation of sugar. This fact has long been known, but only recently has
it been shown that dextrose was the variety of sugar which was formed.
On diluting the strong acid solution with water there is precipitated
out the hydro or oxycelluloses that have been formed, while the
cellulose sulphates are retained in solution.

By suitable means the calcium, barium, or lead salts of these
cellulose-sulphuric acids can be prepared. Analysis of them shows that
these salts undergo hydrolysis, and lose half their sulphuric acid.

The action of strong sulphuric acid has a practical application in the
production of parchment paper; unsized paper is immersed in strong acid
of the proper strength for about a minute, and then immediately rinsed
in water. The acid acts upon the surface of the paper and forms the
cellulose-sulphuric acid which remains attached to the surface. On
passing into the water this is decomposed, the acid is washed away, and
the cellulose is deposited in an amorphous form on the paper, filling up
its pores and rendering it waterproof and grease-proof. Such papers are
now largely used for packing purposes.

ACTION OF HYDROCHLORIC ACID.

Dilute hydrochloric acid of from 1° to 2° Tw. in strength, used in the
cold, has no action on cellulose. Cotton immersed in acids of the
strength named and then well washed in water is not materially affected
in any way, which is a feature of some value in connection with the
bleaching of cotton, where the material has to be treated at two points
in the process with weak acids. Boiling dilute hydrochloric acid of 10°
Tw. disintegrates cellulose very rapidly. The product is a white very
friable powder, which if viewed under the microscope appears to be
fragments of the fibre that has been used to prepare it. The product has
the composition C{12}H{22}O{11}, and is therefore a hydrate of
cellulose, the latter having undergone hydrolysis by taking up the
elements of water according to the equation 2C{6}H{10}O{5} + H{2}O
= C{12}H{22}O{11}. By further digestion with the acid, the
hydrocellulose, as it is called, undergoes molecular change, and is
converted into dextrine. In composition hydrocellulose resembles the
product formed by the addition of sulphuric acid which has received the
name of amyloid. It differs from cellulose in containing free carboxyl,
CO, groups, while its hydroxyl groups, HO, are much more active in their
chemical reactions.

Hydrocellulose is soluble in nitric acid, 1.5 specific gravity, without
undergoing oxidation. Nitrates are formed varying in composition.

The formation of hydrocellulose has a very important bearing in woollen
manufacture. It is practically impossible to obtain wool free from
vegetable fibres, and it is often desirable to separate these vegetable
fibres. For this purpose the goods are passed into a bath of
hydrochloric acid or of weak sulphuric acid. On drying the acid converts
the cotton or vegetable fibre into hydrocellulose which, being friable
or powdery, can be easily removed, while the wool not having been acted
on by the acid remains quite intact. The process is known as
"carbonising". It may not only be done by means of the acids named but
also by the use of acid salts, such as aluminium chloride, which on
being heated are decomposed into free acid and basic oxide. For the same
reason it is important to avoid the use of these bodies, aluminium
chloride and sulphate, zinc and magnesium chlorides, etc., in the
treatment of cotton fabrics; as in finishing processes, where the goods
are dried afterwards, there is a great liability to form hydrocellulose
with the accompaniment of the tendering of the goods.

ACTION OF NITRIC ACID.

The action of nitric acid on cellulose is a variable one, depending on
many factors, strength of acid, duration of action and temperature.
Naturally as nitric acid is a strong oxidising agent the action of
nitric acid on cellulose is essentially in all cases that of an oxidant,
but the character of the product which is obtained varies very much
according to the conditions just noted. When cellulose or cotton in any
form is immersed in nitric acid of 1.4 to 1.5 specific gravity for a
moment, and the fibre be well washed, there is a formation of hydrate of
cellulose which has a gelatinous nature. This is deposited on the rest
of the material, which is not materially affected so far as regards
strength and appearance, but its power of affinity for dyes is
materially increased. There is some shrinkage in the size of the cotton
or paper acted upon.

Nitric acid changes all kinds of cellulose into nitro products, the
composition of which depends upon the strength of the acid, the duration
of treatment, and one or two other factors. The nitrocelluloses are all
highly inflammable bodies, the more highly nitrated burning with
explosive force. They are produced commercially and are known as "gun
cotton" or "pyroxyline". The most highly nitrated body forms the basis
of the explosive variety; the least highly nitrated forms that of the
soluble gun cotton used for making collodion for photographic and other
purposes.

The products formed by the action of nitric acid are usually considered
to be nitrocelluloses. It would appear that they are more correctly
described as cellulose-nitrates, for analysis indicates the presence of
the NO{3} group, which is characteristic of nitrates, and not of the
NO{2} group, which is the feature of nitro bodies in general. Further,
nitro compounds, when subject to the action of reducing agents, are
converted into amido compounds, as is the case, for instance, with
nitro-benzene, C{6}H{5}NO{2}, into aniline, C{6}H{5}NH{2}, or with
nitro-naphthalene, C{10}H{7}NO{2}, which changes into naphthylamine,
C{10}H{7}NH{2}.

But the nitric acid derivatives of cellulose are not capable of
conversion by reducing agents into similar amido compounds. They have
the following properties, which accord more closely with nitrates than
with nitric bodies: alkalies remove the nitric acid; cold sulphuric acid
expels the nitric acid, cellulose sulphates being formed; boiling with
ferrous sulphate and hydrochloric acid causes the elimination of the
nitric acid as nitric oxide (on which reaction a method for determining
the degree of nitration of gun cotton is based). It is best therefore to
consider them as cellulose nitrates. Several well-characterised
cellulose nitrates have been prepared, but is an exceedingly difficult
matter to obtain any one in a state of purity, the commercial articles
being always mixtures of two or three. Those that are best known and of
the most importance are the following:--

Cellulose Hexa-nitrate, C{6}H{4}O{5}(NO{3}){6}. This forms the
principal portion of the commercial explosive gun cotton, and is made
when a mixture of strong nitric acid and strong sulphuric acid is
allowed to act on cotton at from 50 to 55° F. for twenty-four hours. The
longer the action is prolonged, the more completely is the cotton
converted into the nitrate, with a short duration the finished product
contains lower nitrates. This hexa-nitrate is insoluble in ether,
alcohol, or in a mixture of those solvents, likewise in glacial acetic
acid or in methyl alcohol.

Cellulose Penta-nitrate, C{6}H{5}O{5}(NO{3}){5}, is found in
explosive gun cotton to a small extent. When gun cotton is dissolved in
nitric acid and sulphuric acid is added, the penta-nitrate is thrown
down as a precipitate. It is not soluble in alcohol, but is so in a
mixture of ether and alcohol, it is also slightly soluble in acetic
acid. Solutions of caustic potash convert it into the di-nitrate.

Cellulose Tetra-nitrate, C{6}H{6}O{5}(NO{3}){4}, and Cellulose
Tri-nitrate, C{6}H{7}O{5},(NO{3}){3}, form the basis of the
pyroxyline or soluble gun cotton of commerce. It has not been found
possible to separate them owing to their behaviour to solvents being
very similar. These nitrates are obtained by treating cotton with nitric
acid for twenty or thirty minutes. They are characterised by being more
soluble than the higher nitrates and less inflammable. They are freely
soluble in a mixture of ether and alcohol, from which solutions they are
precipitated in a gelatinous form on adding chloroform. Acetic ether,
methyl alcohol, acetone and glacial acetic acid, will also dissolve
these nitrates.

Cellulose Di-nitrate, C{6}H{8}O{5}(NO{3}){2}, is obtained when
cellulose is treated with hot dilute nitric acid, or when the high
nitrates are boiled with solutions of caustic soda or caustic potash.
Like the last-mentioned nitrates it is soluble in a mixture of alcohol
and ether, in acetic ether, and in absolute alcohol. The solution of the
pyroxyline nitrates in ether and alcohol is known as collodion, and is
used in photography and in medical and surgical work.

One of the most interesting applications of the cellulose nitrates is in
the production of artificial silk. Several processes, the differences
between which are partly chemical and partly mechanical, have been
patented for the production of artificial silk, those of Lehner and of
Chardonnet being of most importance. They all depend upon the fact that
when a solution of cellulose nitrate is forced through a fine aperture
or tube, the solvent evaporates almost immediately, leaving a gelatinous
thread of the cellulose nitrate which is very tough and elastic, and
possesses a brilliant lustre. Chardonnet dissolves the cellulose nitrate
in a mixture of alcohol and ether, and the solution is forced through
fine capillary tubes into hot water, when the solvents immediately
evaporate, leaving the cellulose nitrate in the form of very fine fibre,
which by suitable machinery is drawn away as fast as it is formed.
Lehner's process is very similar to that of Chardonnet. Lehner uses a
solution of cellulose nitrate in ether and alcohol, and adds a small
quantity of sulphuric acid; by the adoption of the latter ingredient he
is able to use a stronger solution of cellulose nitrate, 10 to 15 per
cent., than would otherwise be possible, and thereby obtains a stronger
thread which resists the process of drawing much better than is the case
when only a weak solution in alcohol and ether is employed. By
subsequent treatment the fibre can be denitrated and so rendered less
inflammable.

The denitrated fibres thus prepared very closely resemble silk in their
lustre; they are not quite so soft and supple, nor are they in any way
so strong as ordinary silk fibre of the same diameter.

Artificial silk can be dyed in the same manner as ordinary silk.

ACTION OF OXIDISING AGENTS ON CELLULOSE OR COTTON

Cellulose resists fairly well the action of weak oxidising agents; still
too prolonged an action of weak oxidising agents has some influence upon
the cotton fibre, and it may be worth while to point out the action of
some bodies having an oxidising effect.

Nitric acid of about 1.15 specific gravity has little action in the
cold, and only slowly on it when heated. The action is one of oxidation,
the cellulose being transformed into a substance known as oxycellulose.
This oxycellulose is white and flocculent. It tends to form gelatinous
hydrates with water, and has a composition corresponding to the formula
C{6}H{10}O{6}. It is soluble in a mixture of nitric and sulphuric
acids, and on diluting this solution with water a tri-nitrate
precipitates out. A weak solution of soda dissolves this oxycellulose
with a yellow colour, while strong sulphuric acid forms a pink
colouration. It is important to note that nitric acid of the strength
given does not convert all the cellulose into oxycellulose, but there
are formed also carbonic and oxalic acids. When cotton is passed into
strong solutions of bleaching powder and of alkaline hypochlorites and
then dried, it is found to be tendered very considerably. This effect of
bleaching powder was first observed some thirteen years ago by George
Witz, who ascribed the tendering of the cotton to the formation of an
oxycellulose. Although the composition of this particular oxycellulose
so formed has not yet been ascertained, there is reason to think that it
differs somewhat from the oxycellulose formed by the action of the weak
nitric acid. A notable property of the oxycellulose now under
consideration is its affinity for the basic coal-tar dyes, which it will
absorb directly. The oxycellulose is soluble in alkaline solutions.

In the ordinary bleaching process there is considerable risk of the
formation of oxycellulose by the employment of the bleaching solutions
of too great a strength, or in allowing the goods to lie too long before
the final washing off. The presence of any oxycellulose in bleached
cotton may be readily determined by immersing it in a weak solution of
Methylene blue, when, if there be any oxycellulose present, the fibre
will take up some of the dye-stuff.

Permanganate of potash is a very powerful oxidising agent. On cellulose
neutral solutions have but little action, either in the cold or when
heated. They may, therefore, be used for the bleaching of cotton or
other cellulose fibres.

Alkaline solutions of permanganate convert the cellulose into
oxycellulose, which resembles the oxycellulose obtained by the action of
the nitric acid.

Chromic acid, when used in the form of a solution, has but little action
on cellulose. In the presence of mineral acids, and used warm or
boiling, chromic acid oxidises cellulose into oxycellulose and other
products.

It is therefore always advisable in carrying out any technical process
connected with cotton which involves its treatment with oxidising agents
of any kind, and where it is desired not to alter the cotton, to allow
these actions to be as short as possible.

=Dyes and Cotton Dyeing.=--An account of the chemistry of the cotton
fibre would not be complete unless something is said about the reactions
involved in the processes of dyeing and printing cotton. This is a most
interesting subject and opens up quite a number of problems relating to
the combination of the fibre with colouring matter of various kinds, but
here only a brief outline of the principles that present themselves in
considering the behaviour of the cotton fibre as regards colouring
matter will be given.

When the question is considered from a broad point of view, and having
regard to the various affinities of the dyes for cotton; we notice (1)
that there is a large number of dye-stuffs--the Benzo, Congo, Diamine,
Titan, Mikado, etc., dyes--that will dye the cotton from a plain bath or
from a bath containing salt, sodium sulphate, borax or similar salts;
(2) that there are dyes which, like Magenta, Safranine, Auramine and
Methyl violet, will not dye the cotton fibre direct, but require it to
be mordanted or prepared with tannic acid; (3) that there are some dyes
or rather colouring matters which, like Alizarine, Nitroso-resorcine,
barwood, logwood, etc., require alumina, chrome and iron mordants; (4)
that there are some dyes which, like the azo scarlet and azo colours in
general, cannot be used in cotton dyeing; (5) that there are a few dyes,
_i.e._, indigo, which do not come under this grouping.

From the results of recent investigations into the chemistry of dyeing
it is now considered that for perfect dyeing to take place there must be
formed on the fibre a combination which is called a "colour lake," which
consists of at least two constituents; one of these is the dye-stuff or
the colouring matter itself, the other being either the fibre or a
mordant, if such has to be used. The question of the formation of colour
lakes is one connected with the molecular constitution of the colouring
matter, but much yet remains to be done before the proper functions and
mode of action of the various groups or radicles in the dye-stuffs can
be definitely stated. While the constitution of the dye-stuff is of
importance, that of the substance being dyed is also a factor in the
question of the conditions under which it is applied.

In dealing with the first of the above groups of dyes, the direct dyes,
the colourist is somewhat at a loss to explain in what manner the
combination with the cotton fibre is brought about. The affinity of
cellulose for dyes appears to be so small and its chemical activities so
weak, that to assume the existence of a reaction between the dye-stuff
and the fibre, tending to the formation of a colour lake, seems to be
untenable. Then, again, the chemical composition and constitution of the
dyes of this group are so varied that an explanation which would hold
good for one might not do so for another. The relative fastness of the
dyes against washing and soaping precludes the idea of a merely
mechanical absorption of the dye by the fibre; on the other hand the
great difference in the fastness to soaping and light between the same
dyes on cotton and wool would show that there has not been a true
formation of colour lake.

The dyeing of cotton with the second group of dyes is more easily
explained. The cotton fibre has some affinity for the tannic acid used
in preparing it and absorbs it from the mordanting bath. The tannic acid
has the property of combining with the basic constituents of these dyes
and forms a true colour lake, which is firmly fixed on the fibre. The
colour lake can be formed independently of the fibre by bringing the
tannic acid and the dye into contact with one another.

In the case of the dyes of the third group, the formation of a colour
lake between the metallic oxide and the colouring matter can be readily
demonstrated. In dyeing with these colours the cotton is first of all
impregnated with the mordanting oxide, and afterwards placed in the
dye-bath, the mordant already fixed on the fibre then reacts with the
dye, and absorbs it, thus dyeing the cotton. To some extent the dyeing
of cotton with the basic dyes of the second group and the mordant dyes
of the third group is almost a mechanical one, the cotton fibre taking
no part in it from a chemical point of view, but simply playing the part
of a base or foundation on which the colour lake may be formed. In the
case of the dyes of the fourth group, there being no chemical affinity
of the cotton known for them, these dyes cannot be used in a successful
manner; cotton will, if immersed in a bath containing them, more or less
mechanically take up some of the colour from the liquor, but such colour
can be almost completely washed out again, hence these dyes are not used
in cotton dyeing, although many attempts have been made to render them
available.

Indigo is a dye-stuff that stands by itself. Its combination with the
cotton fibre is chiefly of a physical rather than a chemical nature; it
does not form colour lakes in the same way as Alizarine and Magenta do.

Cellulose can be dissolved by certain metallic solutions and
preparations:--

(1) =Zinc Chloride.=--When cotton or other form of cellulose is heated
with a strong solution, 40 to 50 per cent., it slowly dissolves to a
syrupy liquid. On diluting this liquid with water the cellulose is
thrown down in a gelatinous form, but more or less hydrated, and
containing some zinc oxide, 18 to 25 per cent., in combination.

(2) =Zinc Chloride and Hydrochloric Acid.=--When zinc chloride is
dissolved in hydrochloric acid a liquid is obtained which dissolves
cellulose; on dilution the cellulose is re-precipitated in a hydrated
form. It is worth noting that the solution is not a stable one: on
keeping, the cellulose changes its character and undergoes hydrolysis to
a greater or less extent.

(3) =Ammoniacal Copper.=--When ammonia is added to a solution of copper
sulphate, there is formed at first a pale blue precipitate of copper
hydroxide, which on adding excess of ammonia dissolves to a deep blue
solution--a reaction highly characteristic of copper. The ammoniacal
copper solution thus prepared has, as was first observed by John Mercer,
the property of dissolving cellulose fairly rapidly, even in the cold.

If instead of preparing the ammoniacal copper solution in the manner
indicated above, which results in its containing a neutral ammonium
salt, the copper hydroxide be prepared separately and then dissolved in
ammonia a solution is obtained which is stronger in its action.

The cupra-ammonium solutions of cellulose are by no means stable but
change on keeping. When freshly prepared, the cellulose may be
precipitated from them almost unchanged by the addition of such bodies
as alcohol, sugar and solutions of neutral alkaline salts. On keeping
the cellulose undergoes more or less hydrolysis or even oxidation, for
it has been observed that oxycellulose is formed on prolonged digestion
of cellulose with cupra-ammonium solutions, while there is formed a
fairly large proportion of a nitrite.

On adding lead acetate to the cupra-ammonium solution of cellulose, a
compound of lead oxide and cellulose of somewhat variable composition is
precipitated. It is of interest also to note that on adding metallic
zinc to the cupra-ammonium solution the copper is thrown out and a
solution containing zinc is obtained.

This action of cupra-ammonium solutions on cellulose has been made the
basis for the production of the "Willesden" waterproof cloths. Cotton
cloths or paper are passed through these solutions of various degrees of
strength according to requirements, they are then passed through rollers
which causes the surface to become more compact. There is formed on the
surface of the goods a deposit of a gelatinous nature which makes the
surface more compact, and the fabric becomes waterproof in character
while the copper imparts to them a green colour and acts as a
preservative. The "Willesden" fabrics have been found very useful for a
variety of purposes.

CHAPTER II.

SCOURING AND BLEACHING OF COTTON.

Preparatory to the actual dyeing operations, it is necessary to treat
cotton in any condition--loose cotton, yarn, or piece--so that the
dyeing shall be properly done. Raw cotton contains many impurities,
mechanical and otherwise; cotton yarns accumulate dirt and impurities of
various kinds during the various spinning operations, while in weaving a
piece of cotton cloth it is practically impossible to keep it clean and
free from dirt, etc. Before the cotton can be dyed a perfectly level and
uniform shade, free from dark spots or light patches, these impurities
must be removed, and therefore the cotton is subjected to various
scouring or cleansing operations with the object of effecting this end.
Then again cotton naturally, especially Egyptian cotton, contains a
small quantity of a brown colouring matter, and this would interfere
with the purity of any pale tints of blue, rose, yellow, green, etc.,
which may be dyed on the cotton, and so it becomes necessary to remove
this colour and render the cotton quite bright. This is commonly called
"bleaching". It is these preparatory processes that will be dealt with
in this chapter.

=Scouring Cotton.=--When dark shades--blacks, browns, olives, sages,
greens, etc., are to be dyed it is not needful to subject the cotton to
a bleaching operation, but simply to a scouring by boiling it with soda
or caustic soda. This is very often-carried out in the same machine as
the goods will be dyed in; thus, for instance, in the case of pieces,
they would be charged in a jigger, this would be filled with a liquor
made from soda or from caustic soda, and the pieces run from end to end,
while the liquor is being heated to the boil--usually half to
three-quarters of an hour is sufficient. Then the alkali liquor is run
out, clean water run into the jigger and the pieces washed, after which
the dyes, etc., are run into the jigger and the dyeing done. There is
usually used 2 lb. to 3 lb. of caustic soda, or 3 lb. to 4 lb. of soda
for each 100 lb. of goods so treated.

If the ordinary dyeing machines are not used for this purpose, then the
ordinary bleachers' kiers may be used. These will be described
presently.

=Bleaching of Cotton.=--Cotton is bleached in the form of yarn, or in
the finished pieces. In the latter case the method depends very largely
on the nature of the fabric; it is obvious that fine fabrics, like
muslins or lace curtains, cannot stand the same rough treatment as a
piece of twilled calico will. Then, again, the bleaching process is
varied according to what is going to be done with the goods after they
are bleached; sometimes they are sent out as they leave the
bleach-house; again, they may have to be dyed or printed. In the first
case the bleach need not be of such a perfect character as in the last
case, which again must be more perfect than the second class of bleach.
There may be recognised:--

(1) Market or white bleach.
(2) Dyers or printers' bleach.
(3) Madder bleach.

As the madder bleach is by far the most perfect of the three, and
practically includes the others, this will be described in detail, and
differences between it and the others will be then pointed out. A piece
is subjected to the madder bleach which has afterwards to be printed
with madder or alizarine. Usually in this kind of work the cloths are
printed with mordant colours, and then dyed in a bath of the dye-stuff.
This stains the whole of the piece, and to rid the cloth of the stain
where it has to be left white, it is subjected to a soap bath. Now,
unless the bleach has been thorough, the whites will be more or less
stained permanently, and to avoid this cloths which are to be printed
with alizarine colours are most thoroughly bleached. The madder bleach
of the present day generally includes the following series of
operations:--

(1) Stitching.
(2) Singeing.
(3) Singeing wash.
(4) Lime boil.
(5) Lime sour.
(6) Lye boil.
(7) Resin boil.
(8) Wash.
(9) Chemicing.
(10) White sour.

(1) =Stitching.=--The pieces are fastened together by stitching into one
long rope, which is passed in a continuous manner through all operations
in which such a proceeding is possible. This stitching is done by
machines, the simplest of which is the donkey machine, whereby the ends
of the pieces, which are to be stitched together, are forced by a pair
of cogwheels working together on to the needle carrying a piece of
thread, this is then pulled through and forms a running stitch, a
considerable length of thread being left on each side so as to prevent
as far as possible the pulling asunder of the pieces by an accidental
drawing out of the thread.

Birch's sewing machine is very largely used in bleach works. It consists
essentially of a Wilcox & Gibb machine fitted on a stand so as to be
driven by power. The pieces are carried under the needle by a large
wheel, the periphery of which contains a number of projecting pins that,
engaging in the cloth, carry it along.

There is also a contrivance by which these pieces to be sewn can be kept
stretched, this takes the form of an arm with clips at the end, which
hold one end of the cloth while it is running through the machine. The
clip arrangement is automatic, and just before the end passes under the
needle it is released, and the arm flies back ready for the next piece;
it is, however, not necessary to use this arm always. This machine gives
a chain stitch sufficiently firm to resist a pull in the direction of
the length of the pieces, but giving readily to a pull at the end of the
thread.

The Rayer & Lincoln machine is an American invention, and is much more
complicated than Birch's. It consists of a sewing machine mounted on the
periphery of a large revolving wheel. This carries a number of pins,
which, engaging in the cloth to be stitched, carry it under the needle
of the machine. Besides sewing the pieces together this machine is
fitted with a pair of revolving cutters which trim the ends of the
pieces as they pass through in a neat clean manner. There is also an
arrangement to mark the pieces as they are being stitched. Like Birch's
it produces a chain stitch.

What is important in sewing the ends of pieces together is to get a firm
uniform stitch that lies level with the cloths without any knots
projecting, which would catch in the bleaching machinery during the
processes of bleaching, and this might lead to much damage being done.

Should it be necessary to mark the pieces so that they can be recognised
after bleaching, the best thing to use is printers' ink. Gas tar is also
much used, and is very good for the purpose. Coloured inks do not resist
the bleaching sufficiently well to be used satisfactory. Vermilion and
Indian red are used for reds, yellow ochre is the fastest of the
yellows, there is no blue which will stand the process, and Guignet's
green is the only green that will at all resist the process, umber will
serve for brown. All these colours are used in the form of printing ink.

The next operation is a very important one, which cannot be too
carefully carried out, that is:--

(2) =Singeing.=--For printing bleaches the cloths are singed. This has
for its object the removal from the surface of the cloth of the fine
fibres with which it is covered, and which would, if allowed to remain,
prevent the designs printed on from coming out with sufficient
clearness, giving them a blurred appearance.

Singeing is done in various ways, by passing the cloth over a red-hot
copper plate, or over a red-hot revolving copper cylinder, or through a
coke flame, or through gas flames, and more recently over a rod of
platinum made red hot by electricity.

Plate singeing is the oldest of these methods and is still largely used.
In this method a semi-cylindrical copper plate is heated in a suitable
furnace to a bright red heat, the cloths are rapidly passed over it, and
the loose fibres thereby burnt off. One great trouble is to keep the
plate at one uniform heat over the whole of its surface, some parts will
get hotter than others, and it is only by careful attention to the
firing of the furnace that this can be obtained. To get over these
difficulties Worral introduced a roller singeing machine in which the
plate was replaced by a revolving copper roller, heated by a suitable
furnace; the roller can be kept at a more uniform temperature than the
plate. The singe obtained by the plate and roller is good, the principal
fault being that if the cloths happen to get pressed down too much on
the hot plate the loose ends are not burnt off as they should be. With
both plate and roller the cloths are singed only on one side, and if
both sides require to be singed a second passage is necessary. Both
systems still retain their hold as the principal methods in use,
notwithstanding the introduction of more modern methods.

Singeing by passing the cloths over a row of Bunsen burners has come
largely into use. This has the great advantage of being very cleanly,
and of doing the work very effectually, much more thoroughly than any
other method, which is due to the fact that while in the methods
described above only the loose fibres on the surface are burnt off; with
gas all the loose fibres are burnt off. This is brought about by the gas
flame passing straight through the cloth. It is not necessary to
describe the gas singeing machine in detail. Singeing machines should be
kept scrupulously clean and free from fluff, which is liable to collect
round them, and very liable to fire. Some machines are fitted with a
flue having a powerful draught which carries off this fluff, away from
any source of danger.

(3) =Singeing Wash.=--After being singed the cloths are run through a
washing machine to remove by water as much of the loose charred fibres
as possible. The construction of a washing machine is well known. It
consists of a pair of large wooden rollers set above a trough containing
water and into which a constant stream of water flows. In the trough is
also fixed another wooden roller and the pieces are passed round this
bottom roller and between the top rollers. The cloth is passed through
and round the rollers several times in a spiral form so that it passes
through the water in the trough frequently, which is a great advantage,
as the wash is thus much more effectual. The pressure between the two
top rollers presses out any surplus water. The operation scarcely needs
any further description.

(4) =Lime Boil.=--After the cloth leaves the singeing or grey wash, as
it is often called, it passes through the liming machine, which is made
very similar to the washing machine. In this it passes through milk of
lime, which should be made from freshly slaked lime. The latter maybe
prepared in a pasty form in a stone cistern. The lime used should be of
good quality, free from stones, badly burnt pieces or any other
insoluble material, so that when slaked it should give a fine smooth
pasty mass.

Lime should not be slaked too long before using, as it absorbs carbonic
acid from the atmosphere, whereby carbonate of lime is formed, and this
is useless for liming cloth. The pasty slaked lime may be mixed with
water to form the milk of lime, and this can be run from the cistern in
which it is prepared into the liming machine as it is required; the
supply pipe should be run into the bottom of the trough of the liming
machine and not over the top, in which latter case it may splash on to
the cloths and lead to overliming, which is not to be desired on account
of its liability to rot the cloth. The amount of lime used varies in
different bleachworks, and there is no rule on the subject; about 5 lb.
to 7 lb. of dry lime to 100 lb. of cloth may be taken as a fair quantity
to use.

The lime boil has for its object the removal or rather the
saponification of the resinous and fatty matters present in the grey
cloth, either naturally or which have been added in the process of
weaving, or have got upon the cloth accidentally during the processes of
spinning and weaving. With these bodies the lime forms insoluble lime
soaps; these remain in the cloth, but in a form easily decomposable and
removable by treatment with acids and washing. Soda or potash is not
nearly so good for this first boiling as lime--for what reason is
somewhat uncertain, but probably because they form with the grease in
the cloths soluble soaps, which might float about the kier and
accumulate in places where they are not required and thus lead to
stains, whereas the insoluble lime soap remains where it was formed. The
lime also seems to attack the natural colouring matter of the cotton,
and although the colour of the limed cloth is darker than before
boiling, yet the nature of the colour is so altered that it is more
easily removed in the after processes. Besides these changes the
starchy matters put into the cloth in the sizing are dissolved away.
Great care should be taken to see that the goods are evenly laid in the
kiers, not too tight, or the liquor will not penetrate properly; and not
too slack, or they will float about and get entangled and more or less
damaged. Then again care should be taken, especially when using
low-pressure kiers, to see that the supply of liquor does not get too
low, in which case the goods in the upper part of the kier are liable to
get dry and are tendered thereby. So long as the goods in the kiers are
not allowed to get dry there is no risk of damage; this trouble rarely
arises with the Barlow and injector kiers. The inside of the kiers
should be kept well limed, so that the goods shall not come in contact
with the bare iron or metal of which the kier is constructed, as this
would be very likely to lead to stains being produced which are by no
means easy to remove. It is usual, and it is a good plan with almost all
kinds of kiers, except the Mather and Edmeston kiers, to put a number of
large pebbles or small stones at the bottom of the kier, which serves to
make a false bottom on which the goods rest and through which the liquor
penetrates and flows away. Before using, the stones should be well
washed to free them from dirt and grit.

[Illustration: Fig. 4.--Mather & Platt's Low-pressure Bleaching Kier.]

The lime boil is carried out in what are called "kiers". Many forms of
kiers have been devised, but the one in most general use is that known
as the "injector kier," of which a drawing is given in Fig. 4, of the
form made by Messrs. Mather & Platt of Salford. Injector kiers are made
to work either under a pressure of 40 lb. to 50 lb. of steam per square
inch, when they are called high-pressure kiers, or at a pressure of 15
lb. to 20 lb., when they are called low-pressure kiers. The one shown in
the drawing is intended for low-pressure kiers. The principle of
construction is the same in all, the details varying somewhat with
different makers. Injector kiers consist of a hollow, upright iron
cylinder made of plates riveted together; the top is made to lift off,
but can be fastened down tightly by means of bolts and nuts as shown in
the drawing. From the bottom, and placed centrally, rises a pipe, known
as the puffer pipe; this terminates at the top in a rose arrangement.
The lower end of the pipe is perforated. A jet of steam is sent in at
the bottom of this pipe, and by its force any liquor at the bottom of
the kier is forced up the puffer pipe and distributed in a spray over
any goods which may be in the kier. The liquor ultimately finds its way
to the bottom of the kier ready to be blown up again. This circulation
of the liquor can be maintained for any length of time and through its
agency every part of the goods gets thorough and effectual treatment.

The length of the boil depends upon the kiers; with the open kier about
ten hours are usually given, with the Barlow and injector kiers, working
at a pressure of 40 lb. to 50 lb., six to seven hours are given.

(5) =Lime or Grey Sour.=--After the lime boil, the next operation is
that of the lime sour or grey sour as it is often called to distinguish
it from a subsequent souring. The souring is done in a machine
constructed in the same way as a washing machine; the trough of the
machine is filled with hydrochloric acid at 2° Tw., which is kept ready
prepared in a stone cistern and run into the machine as required (it is
not advisable to use acid stronger than this). After passing through the
sour the goods are piled in a heap on the stillage for a few hours. The
acid attacks the lime soap which was formed during the lime boil,
decomposes it and dissolves out the lime with the formation of calcium
chloride, while the fat of the soap is liberated, the former is washed
away in the subsequent washing, while the latter remains to a large
extent on the goods, and is removed by the lye boil that follows.
Sulphuric acid is not so satisfactory to use for the lime sour as
hydrochloric acid, because it forms with the lime the insoluble sulphate
of calcium, which is difficult to entirely remove from the goods,
whereas the chloride is very soluble and is entirely eliminated from the
goods by the washing that follows.

It is advisable to keep the acid at a uniform strength in the machine.
The Twaddell is here of no use as an indicator of the actual strength,
because the lime which the acid dissolves, while it neutralises and
reduces the strength of the acid, actually raises the Twaddell, under
which circumstance the only safe method is a chemical test. This can be
carried out very simply and with a sufficient degree of accuracy by the
workmen, and if it be done at regular intervals during the souring, and
the supply of the fresh acid be regulated, the sour will be kept at a
more uniform strength and more uniform results will be obtained than if
the souring were done in a more empirical fashion. The test is best and
most easily done as follows:--

Prepare a solution of 1 oz. of the powdered high strength 98 per cent.
caustic soda in 1 pint of water, weighing and measuring these quantities
very carefully. Now take a tall, narrow, white bottle of about 5 oz.
capacity and make a mark on the neck. Fill this bottle with the test
solution.

Now take exactly 5 ozs. of freshly prepared sour of 2° Tw., pour into a
jar, and add carefully some of the soda-test solution until a piece of
cloth dyed with turmeric is turned brown, when the acid is neutralised.
Now make a mark on the bottle of soda to show how much has been used. In
all subsequent tests of the sour 5 ozs. should always take the same
quantity of soda solution; if it takes less it is too weak, if more it
is too strong; the remedy in each case is obvious. It is worth while to
graduate the test bottle for 1°, 3°, 4°, 5° Twaddell, as well as for 2°
Tw. acid.

After the souring it is often the custom to pile the goods on to a
wooden stillage, but the goods should not be left too long so piled up
for they may become dry, either entirely or in parts. In any case, as
the goods dry the acid becomes concentrated and attacks them and makes
them tender, which is not at all desirable. Therefore, if it is not
convenient to proceed with them for some time after souring, they
should be moistened with water from time to time, but it is best to wash
them off at once, whereby they are made ready for the next operation.

(6) =Lye Boil.=--This is, perhaps, the most important operation in the
whole process of bleaching, especially if the cloths are going to be
printed in the so-called madder style with alizarine colours, or
otherwise stains are liable to occur in the final stage, and it is then
sometimes difficult to put the blame for these upon the right shoulders.

In principle the lye boil is simple, consisting in boiling the goods
with a solution of soda ash, or caustic soda. The quantity of ash used
varies in different works, as might naturally be expected; from 170 lb.
to 200 lb. of ash to 10,000 lb. of cloth is a fair proportion to use.
The length of boil averages about four hours, certainly not less than
three should be given, and it is not necessary to give more than five
hours in either ordinary kiers, with central puffer pipe, or in injector
kiers.

Care should be taken to see that the goods are well packed into the
kiers, not too tightly or the lye will fail to penetrate equally all
through, and this is important if a uniform bleach is desired; neither
should they be too loose, or they will float about and get torn. It is
not necessary to be particular about the quantity of water used, except
that it must be sufficient to keep the goods well covered, and still
have enough to keep the circulation energetic. When the water is not
sufficient in amount the goods get somewhat dry; there is then a
liability to tendering, but with plenty of water there is no fear of any
damage being done during a boil with alkali. Some works use caustic soda
instead of soda ash in which case less is required, from 120 lb. to 150
lb. to 10,000 lb. of cloth, otherwise no alteration is made in the mode
of boiling.

This lye boil clears away the fatty and waxy matter left in the goods
after the lime sour, and thus prepares the way for the next boil. There
is no advantage in using caustic soda in this preliminary boil, soda ash
being just as effective and cheaper.

(7) =Resin Boil.=--Following the lye boil is the resin boil which
consists in boiling the goods in a resin soap liquor. This is made as
follows: a soda ash liquor of about 15° to 20° Tw. is prepared, and into
this is thrown resin, broken up into small pieces.

The whole is boiled up until the resin is dissolved, and then as much
more is added in small quantities as the alkali will take up. The soda
liquor should not be much weaker than 20° Tw., it will then be heavier
than the resin which will float on the top, it is found to dissolve
quicker and better than when the liquor is weak, in which case, the
resin would sink to the bottom of the boiler and would there melt into a
single mass difficult to dissolve. The resin soap liquor when made is
ready to be used. The proportions of resin and alkali used in the boil
vary in different works, but, as a rule, the quantities for 10,000 lb.
of goods are 430 lb. of 58 per cent. soda ash, 180 lb. of resin, and 80
lb. of 70 per cent. caustic soda. Too much resin should be avoided, as
it is found that with an excess the whites obtained are not nearly so
good as when the right quantity is used; on the other hand, too little
acts much in the same way. It may be taken that from 1-1/2 to 1-3/4 per
cent. of the weight of the goods is about the right proportion; 1 per
cent. being too little, and 2 per cent. too much. The quantity of soda
used should be rather more than twice that of the resin, from 3-1/2 to 4
per cent. The length of boil is usually about twelve hours in a
low-pressure kier; in a high-pressure kier about seven hours is
sufficient.

What the special function of the resin is in this boil is not
definitely known; but experience, both on a large and small scale,
proves that it is essential to obtaining a good white for alizarine
printing; without it, when the goods are dyed with alizarine after the
mordants have been printed on, they frequently take a brown stain--with
the resin this never or but rarely happens.

(8) =Wash.=--After the lye boils the goods must be washed, and it is
important that this be done in as thorough a manner as possible. With
the object of accomplishing this most thoroughly many washing machines
have been invented, the main idea in all being to bring every part of
the goods into contact with as much water as possible. Bridson's is an
old form, and a very good one, the principle of this machine is to cause
the cloth to pass to and fro, and to flap upon the surface of the water
in the trough of the machine.

Furnival's square beater works on much the same principle, and does its
work effectively. More modern washing machines are those of Birch,
Farmer, Mather & Platt, and Hawthorne, where by the peculiar
construction of the rollers and the use of beaters the cloth is very
effectually washed. These machines are much more economical in the use
of water than the older forms, and yet they do their work as well, if
not better.

(9) =Chemicing.=--This is the actual bleaching operation, familiarly
known as "chemicing," that is, the treatment of the goods with bleaching
powder. The previous operations have resulted in obtaining a cloth free
from grease, natural or acquired, and from other impurities, but it
still has a slight brownish colour. This has to be removed before the
goods can be considered a good white, which it is the aim of every
bleacher they should be.

To get rid of this colour they are subjected to some final operations,
the first of which is now to be considered. The chemicing consists in
running the goods through a weak solution of bleaching powder (chloride
of lime), piling the goods up into heaps, and allowing them to lie
overnight, the next day they are finished. As the cloth has received, or
ought to have received, a thorough bottoming, only a weak bath of chemic
is required, about 1/2 to 1° Tw. is quite sufficient. The solution is
prepared in a stone cistern. There is very little difficulty in making
it, the only precaution necessary is to have the solution quite clear
and free from undissolved particles, for if these get upon the cloth
they will either lead to the production of minute holes, or they may
overbleach the fibre, which in such case will have the power of
attracting excess of colour in any subsequent dyeing process and thus
lead to stains, the origin of which may not be readily grasped at the
first sight.

It is best, therefore, either to allow the solution to settle in the
cistern till quite clear, which is the simplest way, or to filter
through cloth.

The chemicing is best done cold and with weak solution, at 1/2° Tw.
rather than 1° Tw. Warming the liquor increases the rapidity of the
bleaching action, but there is a risk of over-chloring, which must be
avoided as far as possible, because there is then danger of tendering
the fibre, moreover, such over-chlored cloth has an affinity for
colouring matters that is not at all desirable, as it leads to the
production of stains and patches in the dyeing operations. It is much
better, when a single chemicing does not bleach the cloth sufficiently
and give a white, to run the cloth twice through a weak liquor rather
than once through a strong liquor.

Although the chemicing is followed by a sour, which, acting on the
bleaching powder, liberates chlorine that bleaches the fabric, yet the
greatest proportion of the bleaching effect is brought about while the
pieces are being piled up into heaps between the chemicing and the sour.
In this state they should be left for some hours, covered over with a
damp sheet, care being taken that they are not left piled so long as to
become dry, as in this event there is a great risk of tendering the
cloth or fabric; it is, therefore, a good plan to moisten them with a
little water from time to time. They should not be tightly piled up, but
be as loose as possible, so that the air can get to them, as it is the
carbonic acid and other acid vapours in the air, that by acting on the
chemic causes slow liberation of chlorine, which effects the bleaching
of the goods.

(10) =White Sour.=--After the chemicing the goods are treated to a sour,
for which purpose either hydrochloric acid or sulphuric acid may be
used.

Hydrochloric acid possesses the advantage of forming a more soluble salt
of lime (calcium chloride) than does sulphuric acid (calcium sulphate),
and it has a more solvent action upon any traces of iron and other
metallic oxide stains which may be present in the goods. On the other
hand, on account of its fuming properties, it is unpleasant to work
with. The souring is done by passing the goods through an acid liquor at
2° Tw. strong and piling for two or three hours, after which it is
washed. This final washing must be thorough, so that all traces of acid
and chemic are washed out, otherwise there is a tendency for the goods
to acquire a yellowish colouration.

So far the routine has been described of the so-called madder bleach,
the most perfect kind of bleach applied to cotton cloths. Besides this
two other kinds of bleach are distinguished in the trade. Turkey red and
market bleach. The former is used when the cloth or yarn is to be dyed
plain or self-coloured with delicate shades with Alizarine; the latter
is used for cloth sold in the white. As the operations involved in
producing these are identical in their method of manipulation to those
already described, it will only be necessary to give an outline of the
process for each one.

=Turkey Red Bleach=--(1) Rinse through water into a kier and boil for
two hours. (2) Lime boil for three to four hours. The amount of lime
required is rather less than what is used with the madder bleach, from
2-1/2 lb. to 3 lb, lime to each 1 cwt. of goods being quite sufficient.
(3) Souring as in the madder bleach. (4) Lye boil, using about 100 lb.
caustic soda to a ton of goods, and giving ten hours' boil. (5) Second
lye boil using about 50 lb. soda ash to a ton of goods, after which the
goods are well washed. (6) Chemicing as with the madder bleach. (7)
Souring as with the madder bleach, then washing well.

This represents an average process, but almost every bleacher has his
own methods, differing from the above in some of the details and this
applies to all bleaching processes. It is obvious that the details may
be varied to a great extent without changing the principles on which the
process depends.

=Market Bleach=--Here all that requires to be done is to get the cloth
of a sufficient degree of whiteness to please the eye of the customer.
Market bleachers have, however, to deal with a wider range of goods than
is dealt with in the former kinds of bleaches, from very fine muslins to
very heavy sheetings. Now it is obvious from a merely mechanical point
of view, that the former could not stand as rough a process as the
latter, therefore there must be some differences in the details of
muslin bleaching and sheeting bleaching. Then again with goods sold in
the white, it is customary to weave coloured headings or markings, and
as these have to be preserved, to do so will cause some slight
alteration of the details of the bleach with this object. On all these
points it is difficult to lay down general rules because of the very
varying feature of the conditions which are met with by the market
bleacher.

The resin boil may be omitted, only two lye boils being required, and
these need not be so long or of such a searching character as the
corresponding boils of the madder bleach. Outlines of two or three such
processes, which are now in use in bleach works, will serve to show the
general routine of a market bleach. The proportions given are calculated
for 10,000 lb. of goods:--

(1) Lime boil, using 500 lb. of lime, and giving a twelve-hours' boil.
(2) Grey sour, hydrochloric acid of 2° Tw., then wash well.
(3) Lye boil, 100 lb. caustic soda, 70 per cent. solid, ten to twelve
hours' boil; wash.
(4) Second lye boil, 100 lb., 58 per cent. soda ash, twelve-hours' boil.
(5) Chemic, bleaching powder liquor at 1° Tw., boil for three hours;
wash.
(6) White sour, sulphuric acid at 2° Tw.; wash well.

The length of boil with the lime and lyes will depend upon the quality
of the goods, heavy goods will require from two to three hours longer
than will light goods, such as cambrics, the time given above being that
for heavy goods, sheetings, etc.

Another process is the following:--

(1) Lime boil, using 480 lb. lime, and boiling for ten hours.
(2) Grey sour, hydrochloric acid at 2° Tw.; wash.
(3) Lye boil, 300 lb. soda ash, 58 per cent.; 50 lb. caustic soda, 70
per cent., and 30 lb. soft soap, giving ten hours' boil; wash.
(4) Chemic as above.
(5) White sour as above; wash well.

A smaller quantity of lime is used here, but on the other hand the lye
boil is a stronger one. This process gives good results. Some bleachers
do not use lime in their market bleaches, but give two lye boils, in
which case the process becomes:--

(1) Lye boil, using 140 lb. caustic soda, of 70 per cent., giving ten
hours' boil and washing well.
(2) Second lye boil, using 120 lb. soda ash, 58 per cent., and giving
ten hours' boil; wash.
(3) Chemic as above.
(4) White sour as above; wash well.

Light fabrics, such as laces, lace curtains, muslins, etc., cannot stand
the strain of the continuous process, and they are therefore subjected
to a different bleaching process, which varies much at different bleach
works. One method is to lime by steeping for an hour in a weak lime
liquor, using about 2 lb. of lime to 100 lb. of goods; they are then
boiled in the kier for eight hours, after which they are washed. This
washing is done in what are called dash wheels, large hollow wheels, the
interior of each being divided into four compartments. Into these the
goods are put, and the wheel is caused to revolve, while at the same
time a current of water flows with some force into the interior of the
wheel and washes the goods.

The wheels do their work well, and the action being gentle the finest
fabrics can be washed without fear of any damage. It is necessary that
the speed at which they are driven should be such that as the wheel
revolves the goods are thrown from side to side of each compartment; if
the speed be too slow they will simply slide down, and then they do not
get properly washed; on the other hand, if the speed be too great then
centrifugal action comes into play and the goods remain in a stationary
position in the wheels with the same result. As to the amount of
washing, it should be as before. After this washing they are boiled
again in the kier with soda ash, using about 8 lb. ash for 100 lb. goods
and giving seven hours' boil, which, after washing, is followed by a
second boil with 5 lb. ash and 4 lb. soft soap for each 100 lb. of
goods, giving eight hours' boil. They are then washed and entered into
the chemic. The chemicing is done in stone cisterns, which are fitted
with false bottoms, on which the goods can rest, and which allow any
insoluble particles of bleaching powder to settle out and prevent them
from getting on the goods. The liquor is used at the strength of about
1/2° Tw., and the goods are allowed to steep about two hours; they are
then placed in a hydro-extractor and the surplus chemic is whizzed out,
after which they are steeped in sour of hydrochloric acid at 1° Tw.,
kept in a stone cistern, the goods being allowed to steep for two hours.
Next they are washed, well whizzed, passed through a blueing water,
whizzed again, and dried. The remarks made when describing similar
operations of the madder bleach as to the action, testing, etc., of the
chemicals, are equally applicable here.

Another plan of bleaching fine fabrics is shown in outline in the
following scheme:--

(1) Wash; boil in water for two hours.
(2) Boil in soda for five hours, using 80 lb. soda ash of 58 per cent.,
and 30 lb. soft soap for 1,000 lb. of goods.
(3) Second soda boil, using from 40 lb. to 50 lb. soda ash, and 15 lb.
to 20 lb. soft soap, giving four hours' boil; after each soda boil the
goods should be washed.
(4) Chemic, using bleaching powder liquor at 1/2° Tw., allowing them to
steep for two hours, then wash and whiz.
(5) White sour, using hydrochloric acid at 2° Tw., steeping two hours;
wash.

A further extension of the same process is sometimes given for the best
goods, which consists, after the above, in giving:--

(6) A third soda boil, using 25 lb. to 30 lb. soda ash and 15 lb. to 20
lb. soft soap, giving one hour's boil; washing.
(7) Chemic as before.
(8) Sour as before, after which the goods are well washed.

In the bleaching of Nottingham lace curtains for the soda boils there
is used what is called the "dolly," which consists of a large round
wooden tub about 5 feet to 6 feet in diameter and about 2 feet 6 inches
to 3 feet deep; this is made to revolve slowly at about one revolution
per minute. Above the tub on a strong frame are arranged four stampers
or beaters, which are caused to rise and fall by means of cams. The
goods are placed in the tub with the scouring liquors and the dolly is
set in motion, the beaters force the liquor into the goods, and the
revolution of the tub causes the beaters to work on a fresh portion of
the goods at every fall.

This is rather an old-fashioned form of machine, and is being replaced
by more modern forms of boiling kiers. In bleaching certain kinds of
muslins in which the warp threads are double, and in the case of lace
curtains, it is necessary to endeavour to keep the threads as open and
prominent as possible. This cannot be done with the continuous process,
which puts a strain on the threads and thus effaces their individuality.
To avoid this the fabrics have to be dealt with in bundles or lumps, and
on these no strain is put, therefore every thread retains its
individuality. The process above described is applicable.

=Yarn Bleaching.=--Yarn is supplied to the bleacher in two forms: (1)
warps in which the length of the threads may vary from as little as 50
to as much as 5,000 yards; these can be dealt with in much the same
manner as a piece of cloth, that is, a continuous system can be adopted;
(2) hanks, which are too well known to require description. Sometimes
yarn is bleached in the form of cops, but as the results of cop
bleaching are not very satisfactory it is done as little as possible.

=Warp Bleaching.=--The warp, if very long, is doubled two, three or four
times upon itself, so as to reduce its length. Care should be taken that
the ends of the warp are tied together to prevent any chance of
entangling, which would very likely happen if the ends were left loose
to float about. As a rule, warps are not limed, but the adoption of the
liming would assist the bleaching. In outline warp bleaching consists of
the following operations:--

(1) Lye boil, using 30 lb. caustic soda, 70 per cent., and 50 lb. soda
ash, 58 per cent., giving six hours' boil, and washing.
(2) Sweeting, boil with 80 lb. soda ash, 58 per cent., for two hours.
(3) Washing.
(4) Chemicing, bleaching powder liquor at 1° Tw., washing.
(5) Sour, sulphuric acid at 2° Tw,. washing well.
(6) Hydro extracting and drying.

About 2,000 to 3,000 lb. of warps are usually treated at one time.

The machinery used may be the same as that used in the cloth bleach, and
each operation may be conducted in the same manner. In some warp
bleachworks, while the kiers are made in the same way, the other
machines are made differently. The chemicing and souring is done in
strong cisterns provided with a false bottom; in these the warps are
allowed to remain for about two hours. A more complicated form of
chemicing cistern is also in use. This is made of stone, and is provided
with a false bottom. Above is a tank or sieve, as it is called, having a
perforated bottom through which the liquor flows on the warp in the
cistern below.

Under the chemicing cistern is a tank into which the liquor flows, and
from which it is pumped up into the sieve above. A circulation of liquor
is thus kept up during the whole of the operation. Owing to the action
of the chemic or acid on the metal work of the pump there is great wear
and tear of the latter, necessitating frequent repairs. This is a defect
in this form of chemicing machine. For drying the warps a
hydro-extractor is first used to get the surplus liquor from the goods.
This machine is now well known, and is in use in every bleachworks,
where it is familiarly known as the "whiz," and the operation is
generally called whizzing. Hydro-extractors are described under the head
of "Dyeing Machinery".

The actual drying of the warps is done over the "tins" as they are
called. These are a number of large cylinders measuring about 20 inches
in diameter and about--for warp drying--5 feet long. Usually they are
arranged vertically in two tiers, each tier consisting of about five
cylinders, not arranged directly one above another but in a zig-zag
manner, the centres of the first, third and fifth being in one line, and
the centres of the others in another line. The cylinders are made to
revolve by suitable driving mechanism, and into them is sent steam at
about 5 lb. to 10 lb. pressure, which heats up the cylinders, whereby
the warp passing over them is dried. This drying may be partial or
complete, being regulated by the speed at which the warps pass over the
cylinders and by the quantity of steam passed into the same. The quicker
the speed and the smaller the amount of steam, the less the warps are
dried; while, on the other hand, the slower the speed and the larger the
amount and greater the pressure of the steam, the quicker and more
thoroughly are the warps dried. As there is a great deal of water formed
in the cylinders by the condensation of the steam, means are always
provided for carrying off this water, as its retention in the cylinders
often leads to serious results and damage to the machine.

=Hank Bleaching.=--So far as the chemical part of hank bleaching is
concerned it does not differ from that of warp bleaching; the same
operations and proportions of chemicals may be used and in the same
order, but there is some difference in the machinery which is used. The
hanks may be manipulated in two ways: they may be either kept in
separate hanks, which is the method mostly in vogue in modern
bleach-houses, or they may be linked together in the form of a chain.
In the latter case the operations and the machinery may be the same as
used in the madder bleach, with a few unimportant minor differences. In
the final washing the dumping machine is used, which consists of two
wooden bowls set over a wooden trough containing the wash waters. The
top bowl is covered with a thick layer of rope and merely rests on the
bottom bowl by its own weight, and is driven by friction from the
latter. The chain of hanks passing through between the two bowls has the
surplus liquor squeezed out of it, and as there is considerable increase
in the thickness at the points of linkage between the hanks, when these
pass through the bowls they lift up the top bowl, which, when the thick
places have passed through, falls down with a sudden bump upon the thin
places, and this bumping drives out all the surplus liquor and drives
the liquor itself into the very centre of the hanks, which is sometimes
an advantage.

In modern bleach-houses the chain form is gradually giving place to the
method of bleaching separate hanks, partly because so many improvements
have been made in the hank-bleaching machinery of late years, which
enables bleachers to handle the yarn in the form of separate hanks
better than they could do formerly; and as bleaching in separate hanks
means that the cotton is kept in a more open form, and is thus more
easily penetrated by the various liquors which are used, it follows that
the bleach will be better and more thorough, which is what the bleacher
aims at. At the same time weaker liquors or, what is the same thing,
less material can be used, which means a saving in the cost of the
process. For bleaching yarn in the hank the following process may be
followed with good results:--

(1) Lye boil, using 1,000 lb. yarn, 40 lb. caustic soda of 70 per cent.,
and 50 lb. of soda ash of 58 per cent., giving five to six hours' boil
at low pressure.
(2) Wash through washing machine.
(3) Second lye boil, using 40 lb. soda ash of 58 per cent., and giving
two to three hours' boil, wash again through a washing machine.
(4) Chemic as in warp bleaching.
(5) Sour as in warp bleaching.
(6) Wash well.
(7) Hydro extract and dry.

Sometimes, if the yarn is to be sold in thread form, before the last
operation it passes through another, _viz._, treating with soap and blue
liquors, which will be dealt with presently.

The lye boils are done in the ordinary kiers, and do not call for
further notice, except that in filling the goods into the kiers care
should be taken that while sufficiently loose to permit of the alkaline
liquors penetrating through the hanks properly, yet they should be so
packed that they will not float about and thus become entangled and
damaged.

The washing is nowadays done in a special form of washing machine,
designed to wash the hanks quickly and well with as little expenditure
of labour and washing liquor as possible. There are now several makes of
these washing machines on the market, most of them do their work well,
and it is difficult to say which is the best. Some machines are made to
wash only one bundle at once, while others will do several bundles.
Generally the principle on which they are constructed is the same in
all, a trough containing the ash liquor, over which is suspended a
revolving reel or bobbin, usually made of wood or enamelled iron, the
bobbin being polygonal in form so that it will overcome readily any
resistance the yarn may offer and carry the hank round as it revolves.
The hank dips into the wash liquor in the trough, and as it is drawn
through by the revolution of the bobbin it is washed very effectually.
The moving of the hank opens out the threads, and thus the wash liquor
thoroughly penetrates to every part of the hank, so that a few minutes'
run through this machine thoroughly washes the yarn. A constant stream
of clean water is passed through the trough. This machine may also be
used for soaping and sizing the hanks if required. By extending the
trough in a horizontal direction, and increasing the number of reels or
bobbins, the quantity of material that can be washed at one time can be
extended, although not to an indefinite extent. The workman can start at
one end of the machine and fill all the bobbins with yarn, by the time
he has finished this the first bobbinful will have been washed
sufficiently and can be taken off and replaced with another quantity of
yarn, and thus one by one the bobbins may be emptied and refilled, which
means that a considerable amount of material can be got through in the
course of a day. To avoid the labour of walking to and fro to fill and
refill the bobbins, washing machines are constructed in which the trough
is made in a circular form. The bobbins are placed at the ends of radial
arms which are caused to revolve round over the trough, the workman is
stationed constantly at one part of the circle, and as the arms pass him
in their motion round the trough he takes off the washed hanks and puts
on the unwashed hanks. By this machine he is saved a very considerable
amount of labour, and is able to do his work in a more convenient
manner. The yarn is well washed in such a machine. The trough may be
entire or it may be divided into a number of compartments, each of which
may contain a different kind of wash liquor if necessary. Of course it
goes almost without saying that in all these machines the liquors in
them may be heated up by means of steam pipes if required.

The chemicing and souring of the hanks does not call for special
mention, beyond the fact that these operations are done in the same
manner as warp bleaching. In Fig. 5 is shown Mather & Platt's
yarn-bleaching kier, which is designed to bleach cotton yarn, either in
hanks or in the warp forms, without removing it from the vessel into
which it is first placed. The process is as follows: The hot alkali
solution is circulated by means of a distributing pipe through the
action of an injector or centrifugal pump to scour the yarn; then water
is circulated by means of a centrifugal pump for washing. The chemic and
sour liquors are circulated also by means of pumps, so that without the
slightest disturbance to the yarn it is quickly and economically
bleached.

[Illustration: FIG. 5.--Mather & Platt's Yarn-bleaching Kier.]

STAINS AND DAMAGES IN BLEACHED GOODS.

Some of the stains in bleached goods which are met are beyond the
control of the bleacher to avoid, while others are due to various
defects in the process. Now the subject of stains can only be dealt with
in a very general way, because of the varying manner in which they
arise. The recognition of the particular way in which the stains have
been formed is sometimes difficult to discover. First, there are iron
stains, which are the most common kind of stains that a bleacher is
troubled with. These generally make their appearance in the form of red
spots of greater or less extent. As a rule they are not visible before
the pieces are fully bleached. Their origin is varied. Sometimes they
arise from the machinery; if the kiers are not kept thoroughly
whitewashed out, there is a great liability to produce iron stains.
Every other machine which is used in the process is made of iron, and
should be kept free from rust, or the chances of stains are considerably
increased. The water used in the bleaching must be free from iron. A
small trace will not make much difference, but some waters contain a
great deal of iron, so much so that they are absolutely unusable for
bleaching purposes. Iron stains are often due to a very curious cause:
the dropping of the oil used in the spinning or weaving machinery on to
the cotton during the process of manufacture. This oil is often charged
with iron derived from the wear and tear of the machinery, and which
often gets fixed in the form of red spots of oxide on the fibre. Iron
stains cannot readily be extracted.

Oil stains are also common. These take the form of bright yellow stains
in various shapes, sometimes extending along the piece in streaks, at
other times in patches in various places about the piece. Generally
these oil stains do not make their appearance as soon as the piece is
bleached, and often the bleacher sends out his goods quite white and
apparently all right, and yet soon afterwards comes a complaint that the
goods are stained yellow. One cause of these yellow oil stains can be
traced to the use of paraffin wax in the sizing of the warps. In this
case the stains are more or less streaky in form, and extend along the
length of the piece. They are due to the fact that paraffin wax is not
saponifiable by the action of the alkalies used in the process, and is
therefore not extracted. When the goods are chemiced the chlorine acts
upon the paraffin and forms chlorine compounds, which are acted upon by
light, and turn yellow by exposure to that agent and to the atmosphere.
Paraffin, when used for the sizing of warps, may sometimes be completely
extracted from the fabric, but this depends upon the proportion of
tallow or other fat which is used in the composition of the sizing
grease. If the paraffin is only present in small quantities, and the
grease well mixed, then it may be possible to extract all the paraffin
out of the fabric during the bleaching process, but if the paraffin is
in large proportion, or the grease not well mixed, it is scarcely
possible to extract it all out, and stains must be the result. These
stains can hardly be considered the fault of the bleacher, but are due
to the manufacturer of the cloth using cheap sizing compositions on his
warps. There are no means which can be adopted before bleaching to
ascertain whether paraffin exists in the cloth. If found to be present,
the remedy which is the easiest practically is to saturate the cloth
with a little olive oil, or better, pale oleic acid. Allow the fatty
matter to soak well in, and then boil the goods in a little caustic
soda. Another cause of oil stains is the use of mineral oils in the
lubrication of cotton machinery. These mineral oils partake of the
nature of paraffin in their properties, and therefore they are
unsaponifiable by the action of alkalies. Like paraffin wax, they
resist the bleaching process, and much in the same manner produce
stains. Oil stains show themselves in various forms--sometimes as spots.
These may be due to the splashing of oil from the spindles during the
process of spinning, or they may be in patches of a comparatively large
size over the pieces.

These are perhaps due to the oil dropping on to the piece during the
process of weaving when in the loom. The oils used for the lubrication
of spinning and weaving machinery should contain a fair proportion of
some fatty oil, such as olive or rape or cocoanut oil. Not less than 10
per cent. should be used. More would be better, but the cost of course
would be greater and oil is an item with spinners and manufacturers.

Stains are occasionally due to other causes rather too numerous to be
dealt with in detail, and sometimes these stains only appear once in a
lifetime, and often do not make their appearance during the bleaching
process, but only in after dyeing or calico printing processes in
curious ways the causes of which are very baffling to find out.

CHAPTER III.

DYEING MACHINERY AND DYEING MANIPULATIONS.

Cotton is dyed in a variety of forms: raw, loose cotton, partly
manufactured fibre in the form of slubbing or sliver, spun fibres or
yarns wound in cop or bobbin forms, in hanks or skeins and in warps, and
lastly in the form of woven pieces. These different forms necessitate
the employment of different forms of machinery and different modes of
handling; it is evident to the least unobservant that it would be quite
impossible to subject slubbing or sliver to the same treatment as yarn
or cloth, otherwise the slubbing would be destroyed and rendered
valueless.

In the early days all dyeing was done by hand in the simplest possible
contrivances, but during the last quarter of a century there has been a
great development in the quantity of dyeing that has been done, and this
has really necessitated the application of machinery, for hand work
could not possibly cope with the amount of dyeing now done. Consequently
there has been devised during the past two decades a great variety of
machines for dyeing every description of textile fabrics, some have not
been found a practical success for a variety of reasons and have gone
out of use, others have been successful and are in use in dye-works.

HAND DYEING.

[Illustration: FIG. 6.--Rectangular Dye-tank.] [Illustration: FIG.
7.--Round Dye-tub.]

Dyeing by hand is carried on in the simplest possible appliances; much
depends upon whether the work can be done at the ordinary temperature
or at the boil. Figs. 6 and 7 show respectively a rectangular vat and a
round tub much in use in dye-houses. These are made of wood, but
copper dye-vats are also made. These may be used for all kinds of
material, loose fibre, yarns or cloth. In the case of loose fibre this
is stirred about either with poles or with rakes, care being taken to
turn every part over and over and open out the masses of fibre as much
as possible in order to avoid matting or clotting together. In the case
of yarns or skeins, these are hung on sticks resting on the edges of the
tub or vat. These sticks are best made of hickory, but ash or beech or
any hard wood that can be worked smooth and which does not swell much
when treated with water may be used. The usual method of working is to
hang the skein on the stick, spreading it out as much as possible, then
immerse the yarn in the liquor, lift it up and down two or three times
to fully wet out the yarn, then turn the yarn over on the stick and
repeat the dipping processes, then allow to steep in the dye-liquor.
This is done with the batch of yarn that is to be dyed at a time. When
all the yarn has been entered into the dye-bath, the first stickful is
lifted out, the yarn turned over and re-entered in the dye-liquor, this
operation is carried out with all the sticks of yarn until the cotton
has become dyed of the required depth. In the case of long rectangular
vats it is customary for two men, one on each side of the vat to turn
the yarns, each man taking charge of the yarn which is nearest to him.
The turning over one lot of yarn is technically called "one turn" and
the dyer often gives "three turns" or "four turns" as may be required.

Woven goods may be dyed in the tub or vat, the pieces being drawn in and
out by poles, but the results are not altogether satisfactory and it is
preferable to use machines for dyeing piece goods.

[Illustration: FIG. 8.--Section of Dye-vat.]

Plain tubs or vats, such as those shown in Figs. 6 and 7, are used for
dyeing, and otherwise treating goods in the cold, or at a lukewarm heat,
when the supply of hot water can be drawn from a separate boiler. When,
however, it is necessary to work at the boil, then the vat must be
fitted with a steam coil. This is best laid along the bottom in a
serpentine form. Above the pipe should be an open lattice-work bottom,
which, while it permits the free circulation of boiling water in the
vat, prevents the material being dyed from coming in contact with the
steam pipe. This is important if uniform shades are to be dyed, for any
excessive heating of any portion of the bath leads to stains being
produced on the material in that part of the bath. Fig. 8 shows a vat
fitted with a steam pipe. That portion of the steam pipe which passes
down at the end of the vat is in a small compartment boxed off from the
main body of the vat, so that no part of the material which is being
dyed can come in contact with it. A closed steam coil will, on the
whole, give the best results, as then no weakening of the dye-liquor can
take place through dilution by the condensation of the steam. Many
dye-vats are, however, fitted with perforated, or, as they are called,
open steam coils, in which case there is, perhaps, better circulation of
the liquor in the dye-vat, but as some of the steam must condense, there
is a little dilution of the dye-liquor in the vat.

DYEING MACHINES.

Dye tubs and vats, such as those described above, have been largely
superseded by machines in which the handling, or working of the
materials being dyed is effected by mechanical means. There have been a
large number of dyeing machines invented, some of these have not been
found to be very practical, and so they have gone out of use. Space will
not admit of a detailed account of every kind of machine, but only of
those which are in constant use in dye-works.

=Dyeing Loose, or Raw Cotton.=--Few machines have been designed for this
purpose, and about the only successful one is:

=Delahunty's Dyeing Machine.=--This is illustrated in Fig. 9. It
consists of a drum made of lattice work, which can revolve inside an
outer wooden casing. The interior of the revolving drum is fitted with
hooks or fingers, whose action is to keep the material open. One segment
of the drum is made to open, so that the loose cotton or wool to be dyed
can be inserted. By suitable gearing the drum can be revolved; and the
dye-liquor, which is in the lower half of the wooden casing, penetrates
through the lattice work of the drum, and dyes the material contained in
it. The construction of the machine is well shown in the drawing, while
the mode of working is obvious from it and the description just given.
The machine is very successful, and well adapted for dyeing loose, or
raw wool and cotton. The material may be scoured, bleached, dyed, or
otherwise treated in this machine.

The Obermaier machine, presently to be described, may also be used for
dyeing loose cotton or wool.

DYEING, SLUBBING, SLIVER OR CARDED COTTON AND WOOL.

[Illustration: FIG. 9.--Delahunty's Dyeing Machine.]

[Illustration: FIG. 10.--Obermaier Dyeing Machine.]

It is found in practice that the dyeing of loose wool or cotton is not
altogether satisfactory--the impurities they naturally contain interfere
with the purity of the shade they will take. Then again the dyes and
mordants used in dyeing them are found to have some action on the wire
of the carding engine through which they are passed; at any rate a card
does not last as long when working dyed cotton or wool as when used on
undyed cotton or wool fibres. Yet for the production of certain fancy
yarns for weaving some special classes of fabrics, it is desirable to
dye the cotton or wool before it is spun into thread. The best plan is
undoubtedly to dye the fibre after it has been carded and partly spun
into what is known as slubbing or sliver. All the impurities have been
removed, the cotton fibres are laid, straight, and so it becomes much
easier to dye. On the other hand, as it is necessary to keep the sliver
or slubbing straight and level, no working about in the dye-liquors can
be allowed to take place, and so such must be dyed in specially
constructed machines, and one of the best of these is the Obermaier
dyeing machine which is illustrated in Fig. 10. The Obermaier apparatus
consists of a dye vat A. In this is placed a cage consisting of an inner
perforated metal cylinder C, and an outer perforated metal cylinder D,
between these two is placed the material to be dyed. C is in contact
with the suction end of a centrifugal pump P, the delivery end of which
discharges into the dye-vat A. The working of the machine is as follows:
The slubbing or sliver is placed in the space between C and D rather
tightly so that it will not move about. Then the inner cage is placed in
the dye-vat as shown. The vat is filled with the dye-liquor which can be
heated up by a steam pipe. The pump is set in motion, the dye liquor is
drawn from A to C, and, in so doing, passes through the material packed
in B and dyes it. The circulation of the liquor is carried on as long as
experience shows to be necessary. The dye-liquor is run off, hot water
is run in to wash the dyed material, and the pump is kept running for
some time to ensure thorough rinsing; then the water is run off, and by
keeping the pump running and air going through a certain amount of
drying can be effected. This machine works very well, and, with a little
experience, constant results can be obtained. The slubbing or sliver may
be scoured, bleached, rinsed, dyed, washed, soaped, or otherwise treated
without removing it from the machine, which is a most decided advantage.

[Illustration: FIG. 11.--Holliday's Yarn-dyeing Machine.]

=Holliday's Yarn-dyeing Machine.=--In Fig. 11 is given an illustration
of a machine for dyeing yarn in the hank form made by Messrs. Read
Holliday & Sons, of Huddersfield. The illustration gives a very good
idea of the machine. It consists of a wooden dye-vat which can be
heated by steam pipes in the usual way. Extending over the vat are a
number of reels or bobbins; these are best made of wood or enamelled
iron; these reels are in connection with suitable gearing so that they
can be revolved. There is also an arrangement by means of which the
reels can be lifted bodily in and out of the dye-vat for the purpose of
taking on and off, "doffing," the hanks of yarn for the reels. A reel
will hold about two pounds of yarn. The working of the machine is
simple. The vat is filled with the requisite dye-liquor. The reels,
which are lifted out of the vat, are then charged with the yarn, which
has been previously wetted out. They are then set in revolution and
dropped into the dye-vat and kept there until it is seen that the yarn
has acquired the desired shade. The reels are lifted out and the hanks
removed, when the machine is ready for another lot of yarn.

There are several makes of hank-dyeing machines of this type, and as a
rule they work very well. The only source of trouble is a slight
tendency for the yarn on one reel if hung loosely of becoming entangled
with the yarn on one of the other reels. This is to some extent obviated
by hanging in the bottom of the hank a roller which acts as a weight and
keeps the yarn stretched and so prevents it flying about.

To some makes of these machines a hank wringer is attached.

[Illustration: FIG. 12.--Klauder-Weldon Dyeing Machine.]

=Klauder-Weldon Hank-dyeing Machine.=--This is illustrated in Fig. 12,
which shows the latest form. This machine consists of a half-cylindrical
dye-vat built of wood. On a central axis is built two discs or rod
carriers which can revolve in the dye-vat, the revolution being given by
suitable gearing, which is shown at the side of the machine. On the
outer edge of the discs are clips for carrying rods, on which one end of
the hanks of yarn is hung, while the other end is placed on a similar
rod carried near the axle. The revolution of the discs carries the yarn
through the dye-liquor contained in the lower semi-cylindrical part of
the machine previously alluded to. At a certain point, every revolution
of the discs, the rods carrying the yarns are turned a little; this
causes the yarn to move on the rods, and this motion helps to bring
about greater evenness of dyeing. The most modern form of this machine
is provided with an arrangement by means of which the whole batch of
yarn can be lifted out of the dye-liquor. Arrangements are made by which
from time to time fresh quantities of dye can be added if required to
bring up the dyed yarn to any desired shade. This machine works well and
gives good results. Beyond the necessary labour in charging and
discharging, and a little attention from time to time, as the operation
proceeds, to see if the dyeing is coming up to shade, the machine
requires little attention.

Many other forms of hank-dyeing machines have been devised: there is
Corron's, in which an ordinary rectangular dye-vat is used. Round this
is a framework which carries a lifting and falling arrangement that
travels to and fro along the vat. The hanks of yarn are hung on rods of
a special construction designed to open them out in a manner as nearly
approaching handwork as is possible. The machine works in this way: the
lifting arrangement is at one end of the vat, the hanks are hung on the
rods and placed in the vat. Then the lifter is set in motion and moves
along the vat; as it does so it lifts up each rod full of yarn, turns it
over, opening out the yarn in so doing, then it drops it again in the
vat. When it has travelled to the end of the vat it returns, picking up
the rods of yarn in so doing, and this motion is kept up until the
dyeing is completed. This machine is very ingenious.

A type of machine which has been made by several makers consists of an
ordinary rectangular dye-vat surrounded with a framework carrying a
number of sets of endless chains, the links of which carry fingers. The
hanks of yarn are hung on rods at one end of which is a tooth wheel that
when in position fits into a rack on the side of the vat. The action of
the machine is this: the hanks are hung on the rods and placed at the
entrance end of the vat, by the moving of the chains it is carried along
the vat and at the same time revolves, thus turning over the yarn which
hangs in the dye-liquor; when it reaches the opposite end of the vat,
the rod full of yarn is lifted out, carried upwards and then towards the
other end of the vat when it is again dropped into the dye-vat to go
through the same cycle of movements which is continued until the yarn is
properly dyed.

COP DYEING.

In weaving fancy-coloured fabrics the ordinary mode is to dye the yarn
in the hank form, then those which have to be used for the weft are
wound into the cop form for placing in the shuttles. The cop form is
that in which the yarn leaves the spinning frame, and necessarily apart
from the dyeing there is labour involved in reeling it into hanks and
winding it back again into the cop form, not only so but there is
necessarily some waste made in these operations. Many attempts have been
made, with more or less success, to dye the yarn while in the cop form
and so save the cost of the hanking and copping above referred to as
well as the waste which occurs. Cops cannot be satisfactorily dyed by
simple immersion in a boiling dye-bath, the outside becomes dyed but the
central portions as often as not remain quite white, and there is a
distinct grading of colour or shade throughout the cop, the outer
portions being deeply dyed while the middle portion will only have a
medium shade and the central portions either not being dyed at all or
only faintly tinted, much depending on the firmness with which the cop
has been wound. A soft, loosely wound cop is much more thoroughly dyed
than a hard, tightly wound cop. This uneven dyeing of the cops is not
satisfactory, and must be avoided if cop dyeing is to be a success. Many
dyers have turned their attention to this question of dyeing yarn in the
cop form, and many machines have been devised for the purpose; some of
these have not been a success, but a few have been found to yield
satisfactory results and proved in practice very successful.

In all machines for dyeing cops one principle has been adopted--that of
drawing or forcing the dye-liquor through the cop.

[Illustration: FIG. 13.--Graemiger Cop-dyeing Machine.]

=Graemiger's Cop-dyeing Machine.=--This is shown in section in Figs. 13
and 14. Although simple in its work it is somewhat complex in its
construction and difficult to describe. The machine consists of a
dye-vat to hold the requisite dye-liquors. In the upper portions of this
is an iron casting formed with four chambers, the two lower ones of
which are immersed in the dye-liquor while the upper chambers are above
it. The sides of this casting are formed of metal plates which fit
tightly against the casting and form as nearly air-and water-tight
joints with it as it is possible to make. These metal plates are on a
spindle and can be rotated. They are perforated and made to carry
spindles, on which are placed the cops to be dyed. The two lower
chambers are in connection with a pump which draws the air from them and
so creates a vacuum inside the chambers. To fill this, liquor from the
dye-vat passes through the cops and into the chambers, and is in turn
drawn through the pump and returned to the dye-vat. In this way there is
a continual circulation of dye-liquors from the vat through the cops,
chambers and pump back to the vat again.

[Illustration: FIG. 14.--Graemiger Cop-dyeing Machine.]

The left upper chamber is practically a blank chamber. Those portions of
the cop carriers in contact with it are filled with cops, which are
placed on perforated spindles; the discs are given a quarter revolution
which brings the cops into the dye-liquor and in connection with the
left lower chamber and are dyed. At the same time the section of the cop
carriers now in contact with the left top chamber is filled with a new
lot of cops, another quarter of a revolution is given to the cop
carriers, which immerse the new lot of cops in the dye-liquor. The third
quarter of the cop plates is filled with cops. A third movement of the
cop plates now takes place; this brings the first lot of cops out of the
dye-liquor and in contact with the right upper chamber, where the
surplus liquor is drawn out of them and returned to the dye-vat. Another
revolution brings the cops back to their first position, they are now
removed and a new lot substituted. These proceedings go on
continuously. Although not quite free from defects the machine gives
very good results, the cops being very uniformly dyed through.

[Illustration: FIG. 15.--- Beaumont's Cop-dyeing Machine.]

=Beaumont's Cop-dyeing Machine.=--This is illustrated in Fig. 15. It
consists of a copper hemispherical dye-vessel, which is provided with a
tightly fitting lid, although this is not needed in all cases. The
bottom of the vessel is in communication with the suction end of a
centrifugal pump, while the delivery end of the pump is attached to the
upper end of the dye-vessel, the action of the pump being to secure a
constant circulation of dye-liquor from the bottom to the top of the
dye-vessel. Arrangements are provided by a peculiar and ingenious
contrivance fitted in one side of the dye-kettle for introducing steam
to heat the dye-liquor to any required degree. As in most forms of
cop-dyeing machines, the cops are placed on perforated metal spindles.
The cops and spindles are inserted in holes in a perforated metal plate,
and over them is placed a thin metal plate, technically called the
antifloater, whose object is to prevent the cops from becoming detached
from the plate. This plate, full of cops, is now placed in the
dye-vessel and rests upon a flange which is provided for that purpose.
When the cop plate is in position the dye-vessel is divided into two
chambers--a lower chamber and an upper one, in the latter being the
cops.

The pump draws liquor from the chamber under the cop plate and so
creates a vacuum, which during the working of the machines ranges from
10 to 20 inches in degree. To supply this vacuum, dye-liquor is drawn
from the upper chamber through the cops. The pump returns the liquor to
the dye-vessel. A very rapid circulation of dye-liquor takes place, from
25 to 50 gallons per minute passing through the cops and pump. From five
to ten minutes is sufficient to dye the cops. The machine is simple in
its construction and gives good results, the cops being completely dyed
through. One important consideration in cop dyeing is to be able to dye
successive batches of cops to exactly the same shade, and this is quite
possible with this machine.

=Young & Crippin's Cop-dyeing Machine.=--So far as simplicity of
construction is concerned this lies between the two preceding machines.
It consists of four parts with some accessory mechanism. There is first
a dye-liquor storage tank at the base of the apparatus in which the
liquor is kept stored and boiling (if necessary) ready for use, above
this and at the front end is the dye-chamber, this communicates at its
lower end by a pipe with the dye-liquor in the dye-vat. Then there is a
large vacuum chamber, in which by means of an injector a vacuum can be
formed, this directly communicates with a liquor-receiving chamber
which again in turn is in

source: Project Gutenberg · page

Cite this

Franklin Beech. "The Dyeing of Cotton Fabrics: A Practical Handbook for the Dyer and Student". Project Gutenberg. Public domain in the USA. https://www.gutenberg.org/ebooks/21224

JSON record · API collection · BibTeX · RIS · CSL-JSON · citation policy