The Automobile Storage Battery: Its Care And Repair
951,988 chars · English
The Project Gutenberg eBook of The Automobile Storage Battery: Its Care And Repair
This eBook is for the use of anyone anywhere in the United States and
most other parts of the world at no cost and with almost no restrictions
whatsoever. You may copy it, give it away or re-use it under the terms
of the Project Gutenberg License included with this eBook or online
at www.gutenberg.org. If you are not located in the United States,
you will have to check the laws of the country where you are located
before using this eBook.
Title: The Automobile Storage Battery: Its Care And Repair
Author: Otto A. Witte
Release date: August 17, 2009 [eBook #29718]
Most recently updated: April 7, 2023
Language: English
Other information and formats: www.gutenberg.org/ebooks/29718
Credits: Produced by George Davis, Mark Posey and Richard Allain
*** START OF THE PROJECT GUTENBERG EBOOK THE AUTOMOBILE STORAGE BATTERY: ITS CARE AND REPAIR ***
Produced by George Davis, Mark Posey and Richard Allain
THE AUTOMOBILE
STORAGE BATTERY
ITS CARE AND REPAIR
------------------------------------------------------------------------
RADIO BATTERIES, FARM LIGHTING BATTERIES
========================================================================
A practical book for the repairman. Gives in nontechnical language,
the theory, construction, operation, manufacture, maintenance, and
repair of the lead-acid battery used on the automobile. Describes at
length all subjects which help the repairman build up a successful
battery repair business. Also contains sections on radio and farm
lighting batteries.
BY
O. A. WITTE
Chief Engineer, American Bureau of Engineering, Inc.
========================================================================
Third Edition
Completely Revised and Enlarged
Fourth Impression
Published 1922 by
THE AMERICAN BUREAU OF ENGINEERING, INC. CHICAGO, ILLINOIS, U. S. A.
Copyright, 1918, 1919, 1920, and 1922, by
American Bureau of Engineering, Inc.
All Rights Reserved.
========================================================================
Entered at Stationers' Hall,
London, England.
First Impression April, 1918.
Second Impression December, 1919.
Third Impression October, 1920.
Fourth Impression September, 1922.
========================================================================
Preface
=======
Many books have been written on Storage Batteries used in stationary
work, as in electric power stations. The storage battery, as used on
the modern gasoline car, however, is subjected to service which is
radically different from that of the battery in stationary work. It is
true that the chemical actions are the same in all lead-acid storage
batteries, but the design, construction, and operation of the starting
and lighting battery, the radio battery, and the farm lighting battery
are unique, and require a special description.
Many books have been written on Storage Batteries used in stationary
work, as in electric power stations. The storage battery, as used on
the modern gasoline car, however, is subjected to service which is
radically different from that of the battery in stationary work. It is
true that the chemical actions are the same in all lead-acid storage
batteries, but the design, construction, and operation of the starting
and lighting battery, the radio battery, and the farm lighting battery
are unique, and require a special description.
This book therefore refers only to the lead-acid type of starting and
lighting battery used on the modern gasoline Automobile, the batteries
used with Radio sets, and the batteries used with Farm Lighting
Plants. It is divided into two sections. The first section covers the
theory, design, operating conditions, and care of the battery.
The second section will be especially valuable to the battery
repairman. All the instructions given have been in actual use for
years, and represent the accumulated experiences of the most
up-to-date battery repair shops in the United States.
The first edition of this book met with a most pleasing reception from
both repairmen and battery manufacturers. It was written to fill the
need for a complete treatise on the Automobile Storage Battery for the
use of battery repairmen. The rapid sale of the book, and the letters
of appreciation from those who read it, proved that such a need
existed.
The automobile battery business is a growing one, and one in which new
designs and processes are continually developed, and in preparing the
second and third editions, this has been kept in mind. Some of the
chapters have been entirely rewritten, and new chapters have been
added to bring the text up-to-date. Old methods have been discarded,
and new ones described. A section on Farm lighting Batteries has been
added, as the automobile battery man should familiarize himself with
such batteries, and be able to repair them. A section on Radio
batteries has also been added.
Special thanks are due those who offered their cooperation in the
preparation and revision of the book. Mr. George M. Howard of the
Electric Storage Battery Co., and Mr. C. L. Merrill of the U. S. Light
& Heat Corporation very kindly gave many helpful suggestions. They
also prepared special articles which have been incorporated in the
book. Mr. Henry E. Peers consulted with the author and gave much
valuable assistance. Mr. Lawrence Pearson of the Philadelphia Battery
Co., Mr. F. S. Armstrong of the Vesta Accumulator Co., Messrs. P. L.
Rittenhouse, E. C. Hicks and W. C. Brooks of the Prest-O-Lite Co., Mr.
D. M. Simpson of the General Lead Batteries Co., Mr. R. D. Mowray and
Mr. C. R. Story of the Universal Battery Co., Mr. H. A. Harvey of the
U. S. Light and Heat Corporation, Mr. E. B. Welsh of the Westinghouse
Union Battery Co., Mr. S. E. Baldwin of the Willard Storage Battery
Co., Mr. H. H. Ketcham of the United Y. M. C. A. Schools, and Messrs.
Guttenberger and Steger of the American Eveready Works also rendered
much valuable assistance.
The Chapter on Business Methods was prepared by Mr. G. W. Hafner.
O. A. WITTE,
Chief Engineer, American Bureau of Engineering, Inc.
September, 1922
========================================================================
Contents
--------
1. INTRODUCTORY
Gasoline and electricity have made possible the modern automobile.
Steps in development of electrical system of automobile. Sources of
electricity on the automobile.
2. BATTERIES IN GENERAL
The Simple Battery, or Voltaic Cell. Chemical Actions which Cause a
Cell to Produce Electricity. Difference between Primary and Secondary,
or Storage Cells. A Storage Battery Does Not "Store" Electricity.
Parts Required to Make a Storage Battery.
3. MANUFACTURE OF STORAGE BATTERIES
Principal Parts of a "Starting and Lighting" Battery. Types of Plates
Used. Molding the Plate Grids. Trimming the Grids. Mixing Pastes.
Applying Pastes to the Plate Grids. Hardening the Paste. Forming the
Plates. Types of Separators. Manufacture of Separators. Manufacture of
Electrolyte. Composition and Manufacture of Jars. Types of Cell
Covers. Single and Double Covers. Covers Using Sealing Compound Around
the Cell Posts. Covers Using Lead Bushings Around the Cell Posts. The
Prest-O-Lite Peened Post Seal. Batteries Using Sealing Nuts Around
Cell Posts. Construction of Vent Tubes. Exide and U. S. L. Vent Tube
Design. Vent Plugs, or Caps. Manufacture of the Battery Case.
Assembling and Sealing the Battery. Terminal Connections. Preparing
the Completed Battery for "Wet" Shipment. Preparing the Completed
Battery for "Dry" Shipment. "Home-Made" Batteries.
4. CHEMICAL CHANGES IN THE BATTERY
Chemical Changes in the Battery. Plante's Work on the Storage Battery.
Faure, or Pasted Plates. How Battery Produces Electricity. Chemical
Actions of Charge and Discharge. Relations Between Chemical Actions
and Electricity.
5. WHAT TAKES PLACE DURING DISCHARGE
What a "Discharge" Consists of. Voltage Changes During Discharge. Why
the Discharge Is Stopped When the Cell Voltage Has Dropped to 1.7 on
Continuous Discharge. Why a Battery May Safely be Discharged to a
Lower Voltage Than 1.7 Volts per Cell at High Rates of Discharge. Why
Battery Voltage, Measured on "Open Circuit" is of Little Value.
Changes in the Density of the Electrolyte. Why Specific Gravity
Readings of the Electrolyte Show the State of Charge of a Cell.
Conditions Which Make Specific Gravity Readings Unreliable. Why the
Specific Gravity of the Electrolyte Falls During Discharge. Why the
Discharge of a Battery Is Stopped When the Specific Gravity Has
Dropped to 1.150. Chemical Changes at the Negative Plates During
Discharge. Chemical Changes at the Positive Plates During Discharge.
6. WHAT TAKES PLACE DURING CHARGE
Voltage Changes During Charge. Voltage of a Fully Charged Cell.
Changes in the Density of the Electrolyte During Charge. Changes at
the Negative Plates During Charge. Changes at the Positive Plates
During Charge.
7. CAPACITY OF STORAGE BATTERIES
Definition of Capacity. Factors Upon Which the Capacity of a Battery
Depend. How the Area of the Plate Surfaces Affects the Capacity. How
the Quantity, Arrangement, and Porosity of the Active Materials Affect
the Capacity. How the Quantity and Strength of the Electrolyte Affect
the Capacity. Why Too Much Electrolyte Injures a Battery. Why the
Proportions of Acid and Water in the Electrolyte Must Be Correct if
Specific Gravity Readings Are to Be Reliable.
8. INTERNAL RESISTANCE
Effect of Internal Resistance. Resistance of Grids. Resistance of
Electrolyte. Resistance of Active Materials.
9. CARE OF BATTERY ON THE CAR
Care of Battery Box. How to Clean the Battery. How to Prevent
Corrosion. Correct Battery Cable Length. Inspection of Battery to
Determine Level of Electrolyte. How to Add Water to Replace
Evaporation. When Water Should Be Added. How Electrolyte Is Lost.
Danger from Adding Acid Instead of Water. Effect of Adding Too Much
Water. When Specific Gravity Readings Should Be Taken. What the
Various Specific Gravity Readings Indicate. Construction of a Syringe
Hydrometer. How to Take Specific Gravity Readings. Why Specific
Gravity Readings Should Not Be Taken Soon After Adding Water to
Replace Evaporation. Troubles Indicated by Specific Gravity Readings.
How to Make Sure That Sections of a Multiple-Section Battery Receive
the Same Charging Current. How Temperature Affects Specific Gravity
Readings. How to Make Temperature Corrections in Specific Gravity
Readings. Battery Operating Temperatures. Effect of Low and High
Temperatures. Troubles Indicated by High Temperatures. Damage Caused
by Allowing Electrolyte to Fall Below Tops of Plates. I-low to Prevent
Freezing. Care of Battery When Not in Use. "Dope" or "Patent"
Electrolyte, or Battery Solutions.
10. STORAGE BATTERY TROUBLES
Normal and Injurious Sulphation.-- How Injurious Sulphate Forms. Why An
Idle Battery Becomes Sulphated. Why Sulphated Plates Must Be Charged
at a Low Rate. How Over discharge Causes Sulphation. How Starvation
Causes Sulphation. How Sulphate Results from Electrolyte Being Below
Tops of Plates. How Impurities Cause Sulphation. How Sulphation
Results from Adding Acid Instead of Water to Replace Evaporation. Why
Adding Acid Causes Specific Gravity Readings to Be Unreliable. How
Overheating Causes Sulphation.
Buckling.-How Overdischarge Causes Buckling. How Continued Operation
with Battery in a Discharged Condition Causes Buckling. I-low Charging
at High Rates Causes Buckling, How Non-Uniform Distribution of Current
Over the Plates Causes Buckling. How Defective Grid Alloy Causes
Buckling.
Shedding, or Loss of Active Material.-- Normal Shedding. How Excessive
Charging Rate, or Overcharging Causes Shedding. How Charging Sulphated
Plates at Too High a Rate Causes Shedding. How Charging Only a Portion
of the Plate Causes Shedding. How Freezing Causes Shedding. How
Overdischarge Causes Loose Active Material. How Buckling Causes Loose
Active Material.
Impurities.-- Impurities Which Cause Only Self-Discharge. Impurities
Which Attack the Plates. How to Remove Impurities. Corroded Grids.-How
Impurities Cause Corroded Grids. How Sulphation Causes Corroded Grids.
How High Temperatures Cause Corroded Grids. How High Specific Gravity
Causes Corroded Grids. How Age Causes Corroded Grids.
Negatives.-- How Age and Heat Cause Granulated Negatives. Heating of
Charged Negatives When Exposed to the Air. Negatives with Very Hard
Active Material. Bulged Negatives. Negatives with Soft, Mushy, Active
Material. Negatives with Rough Surfaces. Blistered Negatives.
Positives.-- Frozen Positives. Rotten, Disintegrated Positives. Buckled
Positives. Positives Which Have Lost Considerable Active Material.
Positives with Soft Active Material. Positives with Hard, Shiny Active
Material. Plates Which Have Been Charged in the Wrong Direction.
Separator Troubles.-- Separators Not Properly Expanded Before
Installation. Improperly Treated Separators. Rotten and Carbonized
Separators. Separators with Clogged Pores. Separators with Edges
Chiseled Off.
Jar Troubles.-- Jars Damaged by Rough Handling. Jars Damaged by Battery
Being Loose. Jars Damaged by Weights Placed on Top of Battery. Jars
Damaged by Freezing of Electrolyte. Jars Damaged by Improperly Trimmed
Plate Groups. Improperly Made Jars. Jars Damaged by Explosions in Cell.
Battery Case Troubles.-- Ends of Case Bulged Out. Rotted Case.
Troubles with Connectors and Terminals.--Corroded and Loose Connectors
and Terminals.
Electrolyte Troubles.-- Low Gravity. High Gravity. Low Level. High
Level. Specific Gravity Does Not Rise During Charge. "Milky"
Electrolyte. Foaming of Electrolyte.
General Battery Troubles.-- Open Circuits. Battery Discharged. Dead
Cells. Battery Will Not Charge. Loss of Capacity. Loss of Charge in an
Idle Battery.
11. SHOP EQUIPMENT
List of Tools and Equipment Required by Repair Shop. Equipment Needed
for Opening Batteries. Equipment for Lead Burning. Equipment for
General Work on Cell Connectors and Terminals. Equipment for Work on
Cases. Tools and Equipment for General Work. Stock. Special Tools.
Charging Equipment. Wiring Diagrams for Charging Resistances and
Charging Circuits. Motor-Generator Sets. Suggestions on Care of
Motor-Generator Sets. Operating the Charging Circuits. Constant
Current Charging. Constant Potential Charging. The Tungar Rectifier.
Principle of Operation of Tungar Rectifier. The Two Ampere Tungar. The
One Battery Tungar. The Two. Battery Tungar. The Four Battery Tungar.
The Ten Battery Tangar. The Twenty Battery Tungar. Table of Tungar
Rectifiers. Installation and Operation of Tungar Rectifier. The
Mercury Are Rectifier. Mechanical Rectifiers. The Stahl Rectifier.
Other Charging Equipment. The Charging Bench. Illustrations and
Working Drawings of Charging Benches. Illustrations and Working
Drawings of Work Benches. Illustrations and Working Drawings of Sink
and Wash Tanks. Lead Burning Outfits. Equipment for Handling Sealing
Compound. Shelving and Racks. Working Drawings of Receiving Racks,
Racks for Repaired Batteries, Racks for New Batteries, Racks for
Rental Batteries, Racks for Batteries in Dry Storage, Racks for
Batteries in "Wet" Storage. Working Drawings of Stock Bins. Working
Drawings for Battery Steamer Bench. Description of Battery Steamer.
Plate Burning Rack. Battery Terminal Tongs. Lead Burning Collars. Post
Builders. Moulds for Casting Lead Parts. Link Combination Mould. Cell
Connector Mould. Production Type Strap Mould. Screw Mould. Battery
Turntable. Separator Cutter. Plate Press. Battery Carrier. Battery
Truck. Cadmium Test Set and How to Make the Test. Paraffine Dip Pot.
Wooden Boxes for Battery Parts. Acid Car boys. Drawing Acid from
Carboys. Shop Layouts. Floor Grating. Seven Architects' Drawings of
Shop Layouts. The Shop Floor. Shop Light.
12. GENERAL SHOP INSTRUCTIONS
Complete instructions for giving a bench charge. Instructions for
Burning Cell Connectors and Terminals. Burning Plates to Strap and
Posts. Post Building. Extending Plate Lugs. Moulding Lead Parts.
Handling and Mixing Acid. Putting New Batteries Into Service (Exide,
Vesta, Philadelphia, Willard, Westinghouse, Prest-O-Lite). Installing
Battery on Car. Wet and Dry Storage of Batteries. Age Codes (Exide,
Philadelphia, Prest-O-Lite, Titan, U.S.L., Vesta, Westinghouse,
Willard). Rental Batteries. Terminals for Rental Batteries. Marking
Chapter Page Rental Batteries. Keeping a Record of Rental Batteries.
General Rental Policy. Radio Batteries. Principles of Audion Bulb for
Radio. Vesta Radio Batteries. Westinghouse Radio Batteries. Willard
Radio Batteries. Universal Radio Batteries. Exide Radio Batteries.
Philadelphia Radio Batteries. U.S.L. Radio Batteries. Prest-O-Lite
Radio Batteries. "Dry" Storage Batteries. Discharge Tests. 15 Seconds
High Rate Discharge Test. 20 Minutes Starting Ability Discharge Test.
"Cycling" Discharge Tests. Discharge Apparatus. Packing Batteries for
Shipping. Safety Precautions for the Repairman. Testing the Electrical
System of a Car. Complete Rules and Instructions for Quickly Testing,
Starting and Lighting System to Protect Battery. Adjusting Generator
Outputs. How and When to Adjust Charging Rate. Re-insulating the
Battery. Testing and Filling Service. Service Records. Illustrations
of Repair Service Record Card. Rental Battery Stock Card.
13. BUSINESS METHODS
Purchasing Methods. Stock Records. The Use and Abuse of Credit. Proper
Bookkeeping Records. Daily Exhibit Record. Statistical and Comparative
Record.
14. WHAT'S WRONG WITH THE BATTERY?
"Service." Calling and Delivering Repaired Batteries. How to Diagnose
Batteries That Come In. Tests on Incoming Batteries. General
Inspection of Incoming Batteries. Operation Tests for Incoming
Batteries. Battery Trouble Charts. Causes of Low Gravity or Low
Voltage. Causes of Unequal Gravity Readings. Causes of High Gravity.
Causes of Low Electrolyte. How to Determine When Battery May Be Left
on Car. How to Determine When Battery Must Be Removed from Car. How to
Determine When It Is Unnecessary to Open a Battery. How to Determine
When Battery Must Be Opened.
15. REBUILDING THE BATTERY
How to Open a Battery.-- Cleaning Outside of Battery Before Opening.
Drilling and Removing Connectors and Terminals. Removing the Sealing
Compound by Steam, Hot Water, Hot Putty Knife, Lead Burning Flame, and
Gasoline Torch. Lifting Plates Out of Jars. Draining Plates. Removing
Covers. Scraping Sealing Compound from the Covers. Scraping Sealing
Compound from Inside of Jars.
What Must Be Done with the Opened Battery?-- Making a Preliminary
Examination of Plates. When to Put in New Plates. When Old Plates May
Be Used Again. What to Do with the Separators. Find the Cause of Every
Trouble. Eliminating "Shorts." Preliminary Charge After Eliminating
Shorts. Washing and Pressing Negatives. Washing Positives. Burning on
New Plates. Testing Jars for Cracks and Holes. Removing Defective
Jars. Repairing the Case.
Reassembling the Elements.-- Putting in Now Separators. Putting
Elements Into Jars. Filling Jars with Electrolyte. Putting Chapter
Page on the Covers. Sealing the Covers. Burning on the Connectors and
Terminals. Marking the Repaired Battery. Cleaning and Painting the
Case. Charging the Rebuilt Battery. Testing.
16. SPECIAL INSTRUCTIONS
Exide Batteries.-- Types. Type Numbers. Methods of Holding Jars in
Case. Opening Exide Batteries. Work on Plates, Separators, Jars, and
Case. Putting Plates in Jars. Filling Jars with Electrolyte. Sealing
Covers. Putting Cells in Case. Burning on the Cell Connectors.
Charging After Repairing. Tables of Exide Batteries.
U.S.L. Batteries.-- Old and New. U.S.L. Covers. Special Repair
Instructions. Tables of U.S.L. Batteries.
Prest-O-Lite Batteries.-- Old and New Prest-O-Lite Cover Constructions.
The "Peened" Post Seal. Special Tools for Work on Prest-O-Lite
Batteries. The Peening Press. Removing Covers. Rebuilding Posts.
Locking, or "Peening" the Posts. Precautions in Post Locking
Operations. Tables of Prest-0-Lite Batteries.
Philadelphia Diamond Grid Batteries.-- Old and New Types. The
Philadelphia "Rubber-Lockt" Cover Seal. Philadelphia Rubber Case
Batteries. The Philadelphia Separator. Special Repair Instructions.
Eveready Batteries.-- Why the Eveready Batteries Are Called
"Non-Sulphating" Batteries. Description of Parts of Eveready Battery.
Special Repair Instructions.
Vesta Batteries.-- Old and New Vesta Isolators. The Vesta Type "D"
Battery. The Vesta Type "DJ" Battery. Vesta Separators. The Vesta Post
Seal. Special Repair Instructions for Old and New Isolators and Post
Seal.
Westinghouse Batteries.-- The Westinghouse Post Seal. Westinghouse
Plates. Types of Westinghouse Batteries. Type "A" Batteries. Type "B"
Batteries. Type "C" Batteries. Type "E" Batteries. Type "H" Batteries.
Type "J" Batteries. Type "0" Batteries. Type "F" Batteries.
Willard Batteries.-- Double and Single Cover Batteries. Batteries with
Sealing Compound Post Seal. Batteries with Lead Inserts in Cover Post
Holes. Batteries with Rubber Casket Post Seal. Special Repair
Instructions for Work on the Different Types of Post Seal
Constructions. Willard Threaded Rubber Separators.
Universal Batteries.-- Types. Construction Features. Putting New
Universal Batteries Into Service.
Titan Batteries.-- The Titan Grid. The Titan Post Seal.
17. FARM LIGHTING BATTERIES
Comparison of Operating Conditions of Farm Lighting Batteries with
Automobile Batteries. Jars for Farm Lighting Batteries. Separators.
Electrolyte. Charging Equipment. Relation of the Automobile Battery
Man to the Farm Lighting Plant. Rules Governing the Selection of a
Farm Lighting Plant. Location and Wiring of Farm Lighting Plant.
Installation. Care of Plant in Service. Care of Battery. Charging Farm
Lighting Batteries. Rules Governing Discharging of Farm Lighting
Batteries. Troubles Found in Farm Lighting Batteries. Inspection and
Tests on Farm Lighting Batteries. Description of Prest-O-Lite Farm
Lighting Battery. Rebuilding Prest-O-Lite Farm Lighting Batteries.
Description of Exide Farm Lighting Batteries. The Delco-Light Battery.
Rebuilding and Repairing Exide Farm Lighting Batteries. Westinghouse
Farm Lighting Batteries. Willard Farm Lighting Batteries.
DEFINITIONS
Condensed Dictionary of Words and Terms Used in Battery Work.
GENERAL INDEX
A VISIT TO THE FACTORY
Photographs showing factory processes.
BUYERS' INDEX. (Omitted.)
For the Convenience of Our Readers We Have Prepared a List of
Companies from Whom Battery Shop Equipment May Be Obtained.
ADVERTISEMENTS (Omitted. Outdated; high bandwidth)
========================================================================
Section I
---------
Working Principles, Manufacture,
Maintenance, Diseases,
and Remedies
========================================================================
The Automobile Storage Battery
========================================================================
CHAPTER 1.
INTRODUCTORY.
Gasoline and electricity have made possible the modern automobile.
Each has its work to do in the operation of the car, and if either
fails to perform its duties, the car cannot move. The action of the
gasoline, and the mechanisms that control it are comparatively simple,
and easily understood, because gasoline is something definite which we
can see and feel, and which can be weighed, or measured in gallons.
Electricity, on the other hand, is invisible, cannot be poured into
cans or tanks, has no odor, and, therefore, nobody knows just what it
is. We can only study the effects of electricity, and the wires,
coils, and similar apparatus in which it is present. It is for this
reason that an air of mystery surrounds electrical things, especially
to the man who has not made a special study of the subject.
Without electricity, there would be no gasoline engine, because
gasoline itself cannot cause the engine to operate. It is only when
the electrical spark explodes or "ignites" the mixture of gasoline and
air which has been drawn into the engine cylinders that the engine
develops power. Thus an electrical ignition system has always been an
essential part of every gasoline automobile.
The first step in the use of electricity on the automobile, in
addition to the ignition system, consisted in the installation of an
electric lighting system to replace the inconvenient oil or gas lamps
which were satisfactory as far as the light they gave was concerned,
but which had the disadvantage of requiring the driver to leave his
seat, and light each lamp separately, often in a strong wind or rain
which consumed many matches, time, and frequently spoiled his temper
for the remainder of the evening. Electric lamps have none of these
disadvantages. They can be controlled from the driver's seat, can be
turned on or off by merely turning or pushing a switch-button, are not
affected by wind or rain, do not smoke up the lenses, and do not send
a stream of unpleasant odors back to the passengers.
The apparatus used to supply the electricity for the lamps consisted
of a generator, or a "storage" battery, or both. The generator alone
had the disadvantage that the lamps could be used only while the
engine was running. The battery, on the other hand, furnished light at
all times, but had to be removed from the car frequently, and
"charged." With both the generator and battery, the lights could be
turned on whether the engine was running or not, and, furthermore, it
was no longer necessary to remove the battery to "charge," or put new
life into it. With a generator and storage battery, moreover, a
reliable source of electricity for ignition was provided, and so we
find dry batteries and magnetos being discarded in a great many
automobiles and "battery ignition" systems substituted.
The development of electric lighting systems increased the popularity
of the automobile, but the motor car still had a great
drawback-cranking. Owing to the peculiar features of a gasoline
engine, it must first be put in motion by some external power before
it will begin to operate under its own power. This made it necessary
for the driver to "crank" the engine, or start it moving, by means of
a handle attached to the engine shaft. Cranking a large engine is
difficult, especially if it is cold, and often results in tired
muscles, and soiled clothes and tempers. It also made it impossible
for the average woman to drive a car because she did not have the
strength necessary to "crank" an engine.
The next step in the perfection of the automobile was naturally the
development of an automatic device to crank the engine, and thus make
the driving of a car a pleasure rather than a task. We find,
therefore, that in 1912, "self-starters" began to be used. These were
not all electrical, some used tanks of compressed air, others
acetylene, and various mechanical devices, such as the spring
starters. The electrical starters, however, proved their superiority
immediately, and filled such a long felt want that all the various
makes of automobiles now have electric starters. The present day motor
car, therefore, uses gasoline for the engine only, but uses
electricity for ignition, starting, lighting, for the horn, cigar
lighters, hand warmers on the steering wheel, gasoline vaporizers, and
even for shifting speed changing gears, and for the brakes.
On any car that uses an electric lighting and starting system, there
are two sources of electricity, the generator and the battery, These
must furnish the power for the starting, or "cranking" motor, the
ignition, the lights, the horn, and the other devices. The demands
made upon the generator are comparatively light and simple, and no
severe work is done by it. The battery, on the other hand is called
upon to give a much more severe service, that of furnishing the power
to crank the engine. It must also perform all the duties of the
generator when the engine is not running, since a generator must be in
motion in order to produce electricity.
A generator is made of iron, copper, carbon, and insulation. These are
all solid substances which can easily be built in any size or shape,
and which undergo very little change as parts of the generator. The
battery is made mainly of lead, lead compounds, water and sulphuric
acid. Here we have liquids as well as solids, which produce
electricity by changes in their composition, resulting in complicated
chemical as well as electrical actions.
[Fig. 1 The Battery]
The battery is, because of its construction and performance, a much
abused, neglected piece of apparatus which is but partly understood,
even by many electrical experts, for to understand it thoroughly
requires a study of chemistry as well as of electricity. Knowledge of
the construction and action of a storage battery is not enough to make
anyone an expert battery man. He must also know how to regulate the
operating conditions so as to obtain the best service from the
battery, and he must be able to make complete repairs on any battery
no matter what its condition may be.
========================================================================
CHAPTER 2.
BATTERIES IN GENERAL
There are two ways of "generating" electricity on the car: 1.
Magnetically, 2. Chemically. The first method is that used in a
generator, in which wires are rotated in a "field" in which magnetic
forces act. The second method is that of the battery, and the one in
which we are now interested.
If two unlike metals or conducting substances are placed in a liquid
which causes a greater chemical change in one of the substances than
in the other, an electrical pressure, or "electromotive" force is
caused to exist between the two metals or conducting substances. The
greater the difference in the chemical action on the substances, the
greater will be the electrical pressure, and if the substances are
connected together outside of the liquid by a wire or other conductor
of electricity, an electric current will flow through the path or
"circuit" consisting of the liquid, the two substances which are
immersed in the liquid, and the external wire or conductor.
As the current flows through the combination of the liquid, and the
substances immersed in it, which is called a voltaic "cell," one or
both of the substances undergo chemical changes which continue until
one of the substances is entirely changed. These chemical changes
produce the electrical pressure which causes the current to flow, and
the flow will continue until one or both of the substances are changed
entirely. This change due to the chemical action may result in the
formation of gases, or of solid compounds. If gases are formed they
escape and are lost. If solids are formed, no material is actually
lost.
Assuming that one of the conducting substances, or "electrodes," which
are immersed in the liquid has been acted upon by the liquid, or
"electrolyte," until no further chemical action can take place, our
voltaic cell will no longer be capable of causing a flow of
electricity. If none of the substances resulting from the original
chemical action have been lost as gases, it may be possible to reverse
the entire set of operations which have taken place. That is, suppose
we now send a current through the cell from an outside source of
electricity, in a direction opposite to that in which the current
produced by the chemical action between the electrodes and electrolyte
flowed. If this current now produces chemical actions between
electrodes and electrolyte which are the reverse of those which
occurred originally, so that finally we have the electrodes and
electrolyte brought back to their original composition and condition,
we have the cell just as it was before we used it for the production
of an electrical pressure. The cell can now again be used as a source
of electricity as long as the electrolyte acts upon the electrodes, or
until it is "discharged" and incapable of any further production of
electrical pressure. Sending a current through a discharged cell, so
as to reverse the chemical actions which brought about the discharged
conditions, is called "charging" the cell.
[Fig. 2 A complete cell; Negative group; Positive group]
Cells in which an electrical pressure is produced as soon as the
electrodes are immersed in the electrolyte are called it "primary"
Cells. In these cells it is often impossible, and always
unsatisfactory to reverse the chemical action as explained above.
Cells whose chemical actions are reversible are called "storage" or
"secondary" cells. In the "storage" cells used today, a current must
first be sent through the cell in order to cause the chemical changes
which result in putting the electrodes and electrolyte, in such a
condition that they will be capable of producing an electrical
pressure when the chemical changes caused by the current are complete.
The cell now possesses all the characteristics of a primary cell, and
may be used as a source of electricity until "discharged." It may then
be "charged" again, and so on, the chemical action in one case causing
a flow of current, and a reversed flow of current causing reversed
chemical actions.
We see from the above that the "storage" battery does not "store"
electricity at all, but changes chemical into electrical energy when
"discharging," and changes electrical into chemical energy when
"charging," the two actions being entirely reversible. The idea of
"storing" electricity comes from the fact that if we send a current of
electricity through the cell for a certain length of time, we can at a
later time draw a current from the cell for almost the same length of
time.
[Fig. 3 Complete Element]
Fig. 3. A complete element, consisting of a positive and negative
group of plates and separators ready for placing in the hard rubber
jars.
Three things are therefore required in a storage cell, the liquid or
"electrolyte" and two unlike substances or electrodes, through which a
current of electricity can pass and which are acted upon by the
electrolyte with a chemical action that is greater for one substance
than the other. In the storage cell used on the automobile today for
starting and lighting, the electrodes are lead and peroxide of lead,
and the electrolyte is a mixture of sulphuric acid and water. The
peroxide of lead electrode is the one upon which the electrolyte has
the greater chemical effect, and it is called the positive or "+"
electrode, because when the battery is sending a. current through an
external circuit, the current flows from this electrode through the
external circuit, and back to the lead electrode, which is called the
negative, or electrode.
When starting and lighting systems were adopted in 1912, storage
batteries had been used for many years in electric power stations.
These were, however, large and heavy, and many difficult problems of
design had to be solved in order to produce a battery capable of
performing the work of cranking the engine, and yet be portable,
light, and small enough to occupy only a very limited space on the
automobile. As a result of these conditions governing the design, the
starting and lighting battery of today is in reality "the giant that
lives in a box." The Electric Storage Battery Company estimates that
one of its types of batteries, which measures only 12-5/8 inches long,
7-3/8 wide, and 9-1/8 high, and weighs only 63-1/2 pounds, can deliver
enough energy to raise itself to a height of 6 miles straight up in
the air. It must be able to do its work quickly at all times, and in
all sorts of weather, with temperatures ranging from below 0° to 100°
Fahrenheit, or even higher.
The starting and lighting battery has therefore been designed to
withstand severe operating conditions. Looking at such a battery on a
car we see a small wooden box in which are placed three or more
"cells," see Fig. 1. Each "cell" has a hard, black rubber top through
which two posts of lead project. Bars of lead connect the posts of one
cell to those of the next. To one of the posts of each end cell is
connected a cable which leads into the car, and through which the
current leaves or enters the battery. At the center of each cell is a
removable rubber plug covering an opening through which communication
is established with the inside of the cell for the purpose of pouring
in water, removing some of the electrolyte to determine the condition
of the battery, or to allow gases formed within the cell to escape.
Looking down through this opening we can see the things needed to form
a storage battery: the electrolyte, and the electrodes or "plates" as
they are called. If we should remove the lead bars connecting one cell
to another, and take off the black cover, we should find that the
posts which project out of the cells are attached to the plates which
are broad and flat, and separated by thin pieces of wood or rubber.,
If we lift out the plates we find that they are connected alternately
to the two lead posts, and that the two outside ones have a gray
color. If we pull the plates out from each Other, we find that the
plates next to the two outside ones, and all other plates connected to
the same lead post as these have a chocolate-brown color. If we remove
the jar of the cell, we find that it is made of hard rubber. Pouring
out the electrolyte we find several ridges which hold the plates off
the bottom of the jar. The pockets formed by these ridges may contain
some soft, muddy substance. Thus we have exposed all the elements of a
cell, posts, plates, "separators," and electrolyte. The gray colored
plates are attached to the "negative" battery post, while the
chocolate-brown colored ones are connected to the "positive" battery
post. Examination will show that each of the plates consists of a
skeleton metallic framework which is filled with the brown or gray
substances. This construction is used to decrease the weight of the
battery. The gray filler material is pure lead in a condition called
"spongy lead." The chocolate-brown filler substance is peroxide of
lead.
We have found nothing but two sets of plates--one of pure lead, the
other of peroxide of lead, and the electrolyte of sulphuric acid and
water. These produce the heavy current necessary to crank the engine.
How this is done, and what the chemical actions within the cell are,
are described in Chapter 4.
========================================================================
CHAPTER 3.
MANUFACTURE OF STORAGE BATTERIES.
---------------------------------
To supply the great number of batteries needed for gasoline
automobiles, large companies have been formed. Each company has its
special and secret processes which it will not reveal to the public.
Only a few companies, however, supply batteries in any considerable
quantities, the great majority of cars being supplied with batteries
made by not more than five or six manufacturers. This greatly reduces
the number of possible different designs in general use today.
The design and dimensions of batteries vary considerably, but the
general constructions are similar. The special processes of the
manufacturers are of no special interest to the repairman, and only a
general description will be given here.
A starting and lighting battery consists of the following principal
parts:
1. Plates
2. Separators
3. Electrolyte
4. Jars
5. Covers
6. Cell Connectors and Terminals
7. Case Plates
Of the two general types of battery plates, Faure and Plante, the
Faure, or pasted type, is universally used on automobiles. In the
manufacture of pasted plates there are several steps which we shall
describe in the order in which they are carried out.
Casting the Grid. The grid is the skeleton of the plate. It performs
the double function of supporting the mechanically weak active
material and of conducting the current. It is made of a lead antimony
alloy which is melted and poured into a mould. Pure lead is too soft
and too easily attacked by the electrolyte, and antimony is added to
give stiffness, and resistance to the action of the electrolyte in the
cell. The amount of antimony used varies in different makes but
probably averages 8 to 10%.
The casting process requires considerable skill, the proper
composition of the metal and the temperature of both metal and moulds
being of great importance in securing perfect grids, which are free
from blowholes, and which have a uniform structure and composition.
Some manufacturers cast two grids simultaneously in each mould, the
two plates being joined to each other along the bottom edge.
Trimming the Grids. When the castings have cooled, they are removed
from the moulds and passed to a press or trimming machine which trims
off the casting gate and the rough edges. The grids are given a rigid
inspection, those having shrunken or missing ribs or other defects
being rejected. The grids are now ready for pasting.
[Fig 4. Grid, Trimmed, and Ready for Pasting]
Fig. 4 shows a grid ready for pasting. The heavy lug at one upper
corner is the conducting lug, for carrying the current to the strap,
Fig. 5, into which the lugs are burned when the battery is assembled.
The straps are provided with posts, to which the intercell connectors
and terminal connectors are attached. The vertical ribs of the grids
extend through the plate, providing mechanical strength and
conductivity, while the small horizontal ribs are at the surface and
in staggered relation on opposite faces. Both the outside frames and
the vertical ribs are reinforced near the lug, where the greatest
amount of current must be carried.
The rectangular arrangement of ribs, as shown in Fig. 4, is most
generally used, although, there are other arrangements such as the
Philadelphia "Diamond" grid in which the ribs form acute angles,
giving diamond shaped openings, as shown in Fig. 6.
Pastes. There are many formulas for the pastes, which are later
converted into active material, and each is considered a trade secret
by the manufacturer using it. The basis of all, however, is oxide of
lead, either Red Lead (Pb30 4), Litharge (PbO), or a mixture of the
two, made into a paste with a liquid, such as dilute sulphuric acid.
The object of mixing the oxides with the liquid is to form a paste of
the proper consistency for application to the grids, and at the same
time introduce the proper amount of binding, or setting agent which
will give porosity, and which will bind together the active material,
especially in the positive plate. Red lead usually predominates in the
positive paste, and litharge in the negative, as this combination
requires the least energy in forming the oxides to active material.
[Fig. 5 Plate Straps and Posts]
The oxides of lead used in preparing the pastes which are applied to
the grids are powders, and in their dry condition could not be applied
to the grids, as they would fall out. Mixing them with a liquid to
make a paste gives them greater coherence and enables them to be
applied to the grids. Sulphuric acid puts the oxides in the desired
pasty condition, but has the disadvantage of causing a chemical action
to take place which changes a considerable portion of the oxides to
lead sulphate, the presence of which makes the paste stiff and
impossible to apply to the grids. When acid is used, it is therefore
necessary to work fast after the oxides are mixed with sulphuric acid
to form the paste.
In addition to the lead oxides, the pastes may contain some binding
material such as ammonium or magnesium sulphate, which tends to bind
the particles of the active material together. The paste used for the
negatives may contain lamp black to give porosity.
Applying the Paste. After the oxides are mixed to a paste they are
applied to the grids. This is done either by hand, or by machine In
the hand pasting process, the pastes are applied from each face of the
grid by means of a wooden paddle or trowel, and are smoothed off flush
with the surface of the ribs of the grid. This work is done quickly in
order that the pastes may not stiffen before they are applied.
U. S. L. plates are pasted in a machine which applies the paste to the
grid, subjecting it at the same time to a pressure which forces it
thoroughly into the grid, and packs it in a dense mass.
Drying the Paste. The freshly pasted plates are now allowed to dry in
the air, or are dried by blowing air over them. In any case, the
pastes set to a hard mass, in which condition the pastes adhere firmly
to the grids. The plates may then be handled without a loss of paste
from the grids.
[Fig. 6 Philadelphia diamond grid]
Forming. The next step is to change the paste of oxides into the
active materials which make a cell operative. This is called "forming"
and is really nothing but a prolonged charge, requiring several days.
In some factories the plates are mounted in tanks, positive and
negative plates alternating as in a cell. The positives are all
connected together in one group and the negatives in another, and
current passed through just as in charging a battery. In other
factories the positives and negatives are formed in separate tanks
against "dummy" electrodes.
The passing of the current slowly changes the mixtures of lead oxide
and lead sulphate, forming brown peroxide of lead (PbO2), on the
positive plate and gray spongy metallic lead on the negative. The
formation by the current of lead peroxide and spongy lead on the
positive and negative plates respectively would take place if the
composition of the two pastes were identical. The difference in the
composition of the paste for positive and negative plates is for the
purpose of securing the properties of porosity and physical condition
best suited to each.
[Fig. 7 Formed plate, ready to be burned to plate connecting
strap]
When the forming process is complete, the plates are washed and dried,
and are then ready for use in the battery. If the grids of two plates
have been cast together, as is done by some manufacturers, these are
now cut apart, and the lugs cut to the proper height. The next step is
to roll, or press the negatives after they are removed from the
forming bath so as to bring the negative paste, which has become
roughened by gassing that occurred during the forming process, flush
with the surface of the ribs of the grid. A sufficient amount of
sulphate is left in the plates to bind together the active material.
Without this sulphate the positive paste would simply be a powder and
when dry would fall out of the grids like dry dust. Fig. 7 shows a
formed plate ready to be burned to the strap.
Separators
In batteries used both for starting and for lighting, separators made
of specially treated wood are largely used. See Fig. 8. The Willard
Company has adopted an insulator made of a rubber fabric pierced by
thousands of cotton threads, each thread being as long as the
separator is thick. The electrolyte is carried through these threads
from one side of the separator to the other by capillary action, the
great number of these threads insuring the rapid diffusion of
electrolyte which is necessary in batteries which are subjected to the
heavy discharge current required in starting.
In batteries used for lighting or ignition, sheets of rubber in which
numerous holes have been drilled are also used, these holes permitting
diffusion to take place rapidly enough to perform the required service
satisfactorily, since the currents involved are much smaller than in
starting motor service.
[Fig. 8]
Fig 8. A Pile of Prepared Wooden Seperators Ready to be Put Between
the Positive and Negative Plates to Form the Complete Element.
For the wooden separators, porous wood, such as Port Orford cedar,
basswood, cypress, or cedar is used. Other woods such as redwood and
cherry are also used. The question is often asked "which wood makes
the best separators?" This is difficult to answer because the method
of treating the wood is just as important as is the kind of wood. The
wood for the separators is cut into strips of the correct thickness.
These strips are passed through a grooving machine which cuts the
grooves in one side, leaving the other side smooth. The strips are
next sawed to the correct size, and are then boiled in a warm alkaline
solution for about 24 hours to neutralize any organic acid, such as
acetic acid, which the wood naturally contains. Such acids would cause
unsatisfactory battery action and damage to the battery.
The Vesta separator, or "impregnated mat," is treated in a bath of
Barium salts which form compounds with the wood and which are said to
make the separators strong and acid-resisting.
[Fig. 9 Philco slotted retainer]
Some batteries use a double separator, one of which is the wooden
separator, while the other consists of a thin sheet of hard rubber
containing many fine perforations. This rubber sheet is placed between
the positive plate and the wooden separator. A recent development in
the use of an auxiliary rubber separator is the Philco slotted
retainer which is placed between the separators and the positives in
Philadelphia Diamond Grid Batteries. Some Exide batteries also use
slotted rubber separators. The Philco slotted retainer consists of a
thin sheet of slotted hard rubber as shown in Fig. 9. The purpose of
the retainer is to hold the positive active material in place and
prevent the shedding which usually occurs. The slots in the retainer
are so numerous that they allow the free passage of electrolyte, but
each slot is made very narrow so as to hold the active material in the
plates.
Electrolyte
Little need be said here about the electrolyte, since a full
description is given elsewhere. See page 222. Acid is received by the
battery manufacturer in concentrated form. Its specific gravity is
then 1.835. The acid commonly used is made by the "contact" process,
in which sulphur dioxide is oxidized to sulphur trioxide, and then,
with the addition of water, changed to sulphuric acid. The
concentrated acid is diluted with distilled water to the proper
specific gravity.
Jars
The jars which contain the plates, separators, and electrolyte are
made of a tough, hard rubber compound. They are made either by the
moulding process, or by wrapping sheets of rubber compound around
metal mandrels. In either case the jar is subsequently vulcanized by
careful heating at the correct temperature.
The battery manufacturers do not, as a rule, make their own jars, but
have them made by the rubber companies who give the jars a high
voltage test to detect any flaws, holes, or cracks which would
subsequently cause a leak. The jars as received at the battery maker's
factory are ready for use.
Across the bottom of the jar are several stiff ribs which extend up
into the jar so as to provide a substantial support for the plates,
and at the same time form several pockets below the plates in which
the sediment resulting from shedding of active material from the
plates accumulates.
Covers
No part of a battery is of greater importance than the hard rubber
cell covers, from the viewpoint of the repairman as well as the
manufacturer. The repairman is concerned chiefly with the methods of
sealing the battery, and no part of his work requires greater skill
than the work on the covers. The manufacturers have developed special
constructions, their aims being to design the cover so as to
facilitate the escape of gas which accumulates in the upper part of a
cell during charge, to provide space for expansion of the electrolyte
as it becomes heated, to simplify inspection and filling with pure
water, to make leak proof joints between the cover and the jar and
between the cover and the lead posts which project through it, and to
simplify the work of making repairs.
Single and Double Covers. Modern types of batteries have a single
piece cover, the edges of which are made so as to form a slot or
channel with the inside of the jar, into which is poured sealing
compound to form a leak proof joint. This construction is illustrated.
in Exide, Fig. 1.5; Vesta, Fig. 264; Philadelphia Diamond Grid, Fig.
256; U. S. L., Figs. 11 and 244; and Prest-0-Lite, Fig. 247,
batteries. Exide batteries are also made with a double flange cover,
in which the top of the jar fits between the two flanges. In single
covers, a comparatively small amount of sealing compound is used, and
repair work is greatly simplified.
In the Eveready battery, Fig. 262, compound is poured over the entire
cover instead of around the edges. This method requires a considerable
amount of sealing compound.
The use of double covers is not as common as it was some years ago.
This construction makes use of two flat pieces of hard rubber. In such
batteries a considerable amount of sealing compound is used. This
compound is poured on top of the lower cover to seal the battery, the
top cover serving to cover up the compound and brace the posts. Fig.
10 illustrates this construction.
[Fig. 10 Cross-section of Gould double cover battery]
Sealing Around the Posts. Much variety is shown in the methods used to
secure a leak proof joint between the posts and the cover. Several
methods are used. One of these uses the sealing compound to make a
tight joint. Another has lead bushings which are screwed up into the
cover or moulded in the cover, the bushings being burned together with
the post and cell connector. Another method has a threaded post, and
uses a lead alloy nut with a rubber washer to make a tight joint.
Still another method forces a lead collar down over the post, and
presses the cover down on a soft rubber gasket.
Using Sealing Compound. Some of the batteries which use sealing
compound to make a tight joint between the cover and the post have a
hard rubber bushing shrunk over the post. This construction is used in
Gould batteries, as shown in Fig. 10, and in the old Willard double
cover batteries. The rubber bushing is grooved horizontally to
increase the length of the sealing surface.
[Fig. 11 U.S.L. cover]
Other batteries that use sealing compound around the posts have
grooves or "petticoats" cut directly in the post and have a well
around the post into which the sealing compound is poured. This is the
construction used in the old Philadelphia Diamond Grid battery, as
shown in Fig. 254.
Using Lead Bushings. U. S. L. batteries have a flanged lead bushing
which is moulded directly into the cover, as shown in Fig. 11. In
assembling the battery, the cover is placed over the post, and the
cell connector is burned to both post and bushing.
[Fig. 12 Lead bushing screwed into cover]
In older type U. S. L. batteries a bushing was screwed up through the
cover, and then burned to the post and cell connector.
An old type Prest-O-Lite battery used a lead bushing which screwed up
through the cover similarly to the U. S. L. batteries. Fig. 12
illustrates this construction. The SJWN and SJRN Willard Batteries
used a lead insert. See page 424.
The modern Vesta batteries use a soft rubber gasket under the cover,
and force a lead collar over the post, which pushes the cover down on
the gasket. The lead collar and post "freeze" together and make an
acid proof joint. See page 413. The Westinghouse battery uses a three
part seal consisting of a lead washer which is placed around the post,
a U shaped, soft gum washer which is placed between the post and
cover, and a tapered lead sleeve, which presses the washer against the
post and the cover. See page 417.
[Fig. 13 Cross section of old type Willard battery]
The Prest-O-Lite Peened Post Seal. All Prest-O-Lite batteries
designated as types WHN, RHN, BHN and JFN, have a single moulded cover
which is locked directly on to the posts. This is done by forcing a
solid ring of lead from a portion of the post down into a chamfer in
the top of the cover. This construction is illustrated in Fig. 247.
Batteries Using Sealing Nuts. The Exide batteries have threaded posts.
A rubber gasket is placed under the cover on a shoulder on the post.
The nut is then turned down on the post to force the cover on the
gasket. This construction is illustrated in Fig. 239. The Titan
battery uses a somewhat similar seal, as shown in Fig. 293.
Some of the older Willard batteries have a chamfer or groove in the
under, side of the cover. The posts have a ring of lead in the base
which fits up into the groove in the cover to make a tight joint.
This is illustrated in Fig. 13. The later Willard constructions, using
a rubber gasket seal and a lead cover insert, are illustrated in Figs.
278 and 287.
Filling Tube or Vent Tube Construction. Quite a number of designs have
been developed in the construction of the filling or vent tube. In
double covers, the tube is sometimes a separate part which is screwed
into the lower cover. In other batteries using double covers, the tube
is an integral part of the cover, as shown in Fig. 10. In all single
covers, the tube is moulded integral with the cover.
[Fig. 14a Vent hold in U.S.L. battery]
Several devices have been developed to make it impossible to overfill
batteries. This has been done by the U. S. L. and Exide companies on
older types of batteries, their constructions being described as
follows:
In old U. S. L. batteries, a small auxiliary vent tube is drilled, as
shown in Fig. 14. When filling to replace evaporation, this vent tube
prevents overfilling.
[Fig. 14b Filling U.S.L. battery]
A finger is placed over the auxiliary vent tube shown in Fig. 14. The
water is then poured in through the filling or vent tube. When the
water reaches the bottom of the tube, the air imprisoned in the
expansion chamber can no longer escape. Consequently the water can
rise no higher in this chamber, but simply fills up the tube. Water is
added till it reaches the top of the tube. The finger is then removed
from the vent tube. This allows the air to escape from the expansion
chamber. The water will therefore fall in the filling or vent tube,
and rise slightly in the expansion chamber. The construction makes it
impossible to overfill the battery, provided that the finger is held
on the vent hole as directed.
[Fig. 14c Filling U.S.L. battery (old types)]
Figure 15 shows the Non-Flooding Vent and Filling Plug used in the
older type Exide battery, and in the present type LXRV. The new Exide
cover, which does not use the non-flooding feature, is also shown. The
old construction is described as follows:
[Fig. 15a Sectional view of cover in older type Exide battery.
Top view of cover and filling plug, plug removed]
[Fig. 15b Old and new Exide covers]
From the illustrations of the vent and filling plug, it will be seen
that they provide both a vented stopper (vents F, G, H), and an
automatic device for the preventing of overfilling and flooding. The
amount of water that can be put into the cell is limited to the exact
amount needed to replace that lost by evaporation. This is
accomplished by means of the hard rubber valve (A) within the cell
cover and with which the top of the vent plug (E) engages, as shown in
the illustrations. The action of removing the plug (E) turns this
valve (A), closing the air passage (BB), and forming an air tight
chamber (C) in the top of the cell. When water is poured in, it cannot
rise in this air space (C) so as to completely fill the cell. As soon
as the proper level is reached, the water rises in the filling tube
(D) and gives a positive indication that sufficient water has been
added. Should, however, the filling be continued, the excess will be
pure water only, not acid. On replacing the plug (E), valve (A) is
automatically turned, opening the air passages (BB), leaving the air
chamber (C) available for the expansion of the solution, which occurs
when the battery is working.
Generally the filling or vent tube is so made that its lower end
indicates the correct level of electrolyte above the plates, In adding
water, the level of the electrolyte is brought up to the bottom of the
filling tube. By looking down into the tube, it can be seen when the
electrolyte reaches the bottom of the tube.
Vent Plugs, or Caps. Vent plugs, or caps, close up the filling or vent
tubes in the covers. They are made of hard rubber, and either screw
into or over the tubes, or are tightened by a full or partial turn, as
is done in Exide batteries. In the caps are small holes which are so
arranged that gases generated within the battery may escape, but acid
spray cannot pass through these holes. It is of the utmost importance
that the holes in the vent caps be kept open to allow the gases to
escape.
Case
The wooden case in which the cells are placed is usually made of kiln
dried white oak or hard maple. The wood is inspected carefully, and
all pieces are rejected that are weather-checked, or contain
worm-holes or knots. The wood is sawed into various thicknesses, and
then cut to the proper lengths and widths. The wood is passed through
other machines that cut in the dovetails, put the tongue on the bottom
for the joints, stamp on the part number, drill the holes for the
screws or bolts holding the handles, cut the grooves for the sealing
compound, etc. The several pieces are then assembled and glued
together. The finishing touches are then put on, these consisting of
cutting the cases to the proper heights, sandpapering the boxes, etc.
The cases are then inspected and are ready to be painted.
A more recent development in case construction is a one-piece hard
rubber case, in which the jars and case are made in one piece, the
cell compartments being formed by rubber partitions which form an
integral part of the case. This construction is used in several makes
of Radio "A" batteries, and to some extent in starting batteries.
[Fig. 16 Exide battery case]
Asphaltum paint is generally used for wooden cases, the bottoms and
tops being given three, coats, and the sides, two. The number of coats
of paint varies, of course, in the different factories. The handles
are then put on by machinery, and the case, Fig. 16, is complete, and
ready for assembling.
Assembling and Sealing
The first step in assembling a battery is to burn the positive and
negative plates to their respective straps, Fig. 5, forming the
positive and negative "groups", Fig. 2. This is done by arranging a
set of plates and a strap in a suitable rack which holds them securely
in proper position, and then melting together the top of the plate
lugs and the portion of the strap into which they fit with a hot flame.
A positive and a negative group are now slipped together and the
separators inserted. The grooved side of the wood separator is placed
toward the positive plate and when perforated rubber sheets are used
these go between the positive and the wood separator. The positive and
negative "groups" assembled with the separators constitute the
"element," Fig. 3.
Before the elements are placed in the jars they are carefully
inspected to make sure that no separator has been left out. For this
purpose the "Exide" elements are subjected to an electrical test which
rings a bell if a separator is missing, this having been found more
infallible than trusting to a man's eyes.
In some batteries, such as the Exide, Vesta, and Prest-O-Lite
batteries, the cover is placed on the element and made fast before the
elements are placed in the jars. In other batteries, such as the U. S.
L. and Philadelphia batteries, the covers are put on after the
elements are placed in the jars.
After the element is in the jar and the cover in position, sealing
compound is applied hot so as to make a leak proof joint between jar
and cover.
[Fig. 17 Inter-cell connector]
The completed cells are now assembled in the case and the cell
connectors, Fig. 17, burned to the strap posts. After filling with
electrolyte the battery is ready to receive its "initial charge,"
which may require from one day to a week. A low charging rate is used,
since the plates are generally in a sulphated condition when
assembled. The specific gravity is brought up to about 1.280 during
this charge. Some makers now give the battery a short high rate
discharge test (see page 266), to disclose any defects, and just
before sending them out give a final charge. The batteries are often
"cycled" after being assembled, this consisting in discharging and
recharging the batteries several times to put the active material in
the best working condition. If the batteries are to be shipped "wet,"
they are ready for shipping after the final charge and inspection.
Batteries which are shipped "dry" need to have more work done upon
them.
Preparing Batteries for Dry Shipment
There are three general methods of "dry" shipment. The first method
consists of sending cases, plates, covers, separators, etc.,
separately, and assembling them in the service stations. Sometimes
these parts are all placed together, as in a finished battery, but
without the separators, the covers not being sealed, or the connectors
and terminals welded to the posts. This is a sort of "knock-down"
condition. The plates used are first fully charged and dried.
The second method consists of assembling a battery complete with
plates, separators, and electrolyte, charging the battery, pouring out
the electrolyte, rinsing with distilled water, pouring out the water
and screwing the vent plugs down tight. The vent holes in these plugs
are sealed to exclude air. The moisture left in the battery when the
rinsing water was poured out cannot evaporate, and the separators are
thus kept in a moistened condition.
The third method is the Willard "Bone Dry" method, and consists of
assembling the battery complete with dry threaded rubber separators
and dry plates, but without electrolyte. The holes in the vent plugs
are not sealed, since there is no moisture in the battery. Batteries
using wooden separators cannot be shipped "bone-dry," since wooden
separators must be kept moist.
Terminal Connections
When the battery is on the car it is necessary to have some form of
detachable connection to the car circuit and this is accomplished by
means of "terminal connectors," Fig. 18, of which there are many types.
[Fig. 18 Battery terminal]
Many types of terminals are in two parts, one being permanently
attached to the car circuit and the other mounted permanently on the
battery by welding it to the terminal post, the two parts being
detachably joined by means of a bolted connection.
In another type of terminal, the cable is soldered directly to the
terminal which is lead burned to the cell post. In this construction
there is very much less chance of corrosion taking place, and it is
therefore a good design.
HOMEMADE BATTERIES
The wisest thing for the battery shop owner to do is to get a contract
as official service station for one of the well known makes of
batteries. The manufacturers of this battery will stand behind the
service station, giving it the benefits of its engineering,
production, and advertising departments, and boost the service
station's business, helping to make it a success.
Within the past year or so, however, some battery repairmen have
conceived the idea that they do not need the backing of a well
organized factory, and have decided to build up their own batteries.
Some of them merely assemble batteries from parts bought from one or
more manufacturers. If all the parts are made by the same company,
they will fit together, and may make a serviceable battery. Often,
however, parts made by several manufacturers are assembled in the same
battery. Here is where trouble is apt to develop, because it is more
than likely that jars may not fit well in the case; plates may not
completely fill the jars, allowing too much acid space, with the
results that specific gravity readings will not be reliable, and the
plates may be overworked; plate posts may not fit the cover holes, and
so on. If such a "fabricated" battery goes dead because of defective
material, there is no factory back of the repairman to stand the loss.
If the repairman wishes to assemble batteries, he should be very
careful to buy the parts from a reliable manufacturer, and he should
be especially careful in buying separators, as improperly treated
separators often develop acetic acid, which dissolves the lead of the
plates very quickly and ruins the battery. Batteries made in this way
are good for rental batteries, or "loaners." These batteries are
assembled and charged just as are batteries which have been in dry
storage, see page 241.
If the repairman who "fabricates" batteries takes chances, the man who
attempts to actually make his own battery plates is certainly risking
his business and reputation. There are several companies which sell
moulds for making plate grids. One even sells cans of lead oxides to
enable the repairman to make his own plate paste. Even more foolhardy
than the man who wishes to mould plate grids is the man who wishes to
mix the lead oxides himself. Many letters asking for paste formulas
have been received by the author. Such formulas can never be given,
for the author does not have them. Paste making is a far more
difficult process than many men realize. The lead oxides which are
used must be tested and analyzed carefully in a chemical laboratory
and the paste formulas varied according to the results of these tests.
The oxides must be carefully weighed, carefully handled, and carefully
analyzed. The battery service station does not have the equipment
necessary to do these things, and no repairman should ever attempt to
make plate paste, as trouble is bound to follow such attempts. A car
owner may buy a worthless battery once, but the next time he will go
to some other service station and buy a good battery.
No doubt many repairmen are as skillful and competent as the workers
in battery factories, but the equipment required to make grids and
paste is much too elaborate and expensive for the service station, and
without such equipment it is impossible to make a good battery.
The only battery parts which may safely be made in the service station
are plate straps and posts, intercell connectors, and cell terminals.
Moulds for making such parts are on the market, and it is really worth
while to invest in a set. The posts made in such moulds are of the
plain tapered type, and posts which have special sealing and locking
devices, such as the Exide, Philadelphia, and Titan cannot be made in
them.
========================================================================
CHAPTER 4.
CHEMICAL CHANGES.
-----------------
Before explaining what happens within one storage cell, let us look
into the early history of the storage battery, and see what a modest
beginning the modern heavy duty battery had. Between 1850 and 1860 a
man named Plante began his work on the storage battery. His original
cell consisted of two plates of metallic lead immersed in dilute
sulphuric acid. The acid formed a thin layer of lead sulphate on each
plate which soon stopped further action on the lead. If a current was
passed through the cell, the lead sulphate on the "anode" or lead
plate at which the current entered the cell was changed into peroxide
of lead, while the sulphate on the other lead plate or "cathode" was
changed into pure lead in a spongy form. This cell was allowed to
stand for several days and was then "discharged," lead sulphate being
again formed on each plate. Each time this cell was charged, more
"spongy" lead and peroxide of lead were formed. These are called the
"active" materials, because it is by the chemical action between them
and the sulphuric acid that the electricity is produced. Evidently,
the more active materials the plates contained, the longer the
chemical action between the acid and active materials could take
place, and hence the greater the "capacity," or amount of electricity
furnished by the cell. The process of charging and discharging the
battery so as to increase the amount of active material, is called
"forming" the plates.
[Fig. 19 Illustration of chemical action in a storage cell
during charge]
Plante's method of forming plates was very slow, tedious, and
expensive. If the spongy lead, and peroxide of lead could be made
quickly from materials which could be spread over the plates, much
time and expense could be saved. It was Faure who first suggested such
a plan, and gave us the "pasted" plate of today, which consists of a
skeleton framework of lead, with the sponge lead and peroxide of lead
filling the spaces between the "ribs" of the framework. Such plates
are known as "pasted" plates, and are much lighter and more
satisfactory, for automobile work than the heavy solid lead plates of
Plante's. Chapter 3 describes more fully the processes of
manufacturing and pasting the plates.
We know now what constitutes a storage battery, and what the parts are
that "generate" the electricity. How is the electricity produced?
Theoretically, if we take a battery which has been entirely
discharged, so that it is no longer able to cause a flow of current,
and examine and test the electrolyte and the materials on the plates,
we shall find that the electrolyte is pure water, and both sets of
plates composed of white lead sulphate. On the other hand, if we make
a similar test and examination of the plates and electrolyte of a
battery through which a current has been sent from some outside
source, such as a generator, until the current can no longer cause
chemical reactions between the plates and electrolyte, we will find
that the electrolyte is now composed of water and Sulphuric acid, the
acid comprising about 30%, and the water 70% of the electrolyte. The
negative set of plates will be composed of pure lead in a spongy form,
while the positive will consist of peroxide of lead.
The foregoing description gives the final products of the chemical
changes that take place in the storage battery. To understand the
changes themselves requires a more detailed investigation. The
substances to be considered in the chemical actions are sulphuric
acid, water, pure lead, lead sulphate, and lead peroxide. With the
exception of pure lead, each of these substances is a chemical
compound, or composed of several elements. Thus sulphuric acid is made
up of two parts of hydrogen, which is a gas; one part of sulphur, a
solid, and four parts of oxygen, which is also a gas; these combine to
form the acid, which is liquid, and which is for convenience written
as H2SO 4, H2 representing two parts of hydrogen, S one part of
sulphur, and 04, four parts oxygen. Similarly, water a liquid, is made
up of two parts of hydrogen and one part of oxygen, represented by the
symbol H2O. Lead is not a compound, but an element whose chemical
symbol is Pb, taken from the Latin name for lead. Lead sulphate is a
solid, and consists of one part of lead, a solid substance, one part
of sulphur, another solid substance, and four parts of oxygen, a gas.
It is represented chemically by Pb SO4. Lead peroxide is also a solid,
and is made up of one part of lead, and two parts of oxygen. In the
chemical changes that take place, the compounds just described are to
a certain extent split up into the substances of which they are
composed. We thus have lead (Pb), hydrogen (H), oxygen (0), and
sulphur (S), four elementary substances, two of which are solids, and
two gases. The sulphur does not separate itself entirely from the
substances with which it forms the compounds H2SO4 and Pb SO4. These
compounds are split into H2 and SO4 and Pb and SO4 respectively. That
is, the sulphur always remains combined with four parts of oxygen.
Let us now consider a single storage cell made up of electrolyte, one
positive plate, and one negative plate. When this cell is fully
charged, or in a condition to produce a current of electricity, the
positive plate is made up of peroxide of lead (PbO2), the negative
plate of pure lead (Pb), and the electrolyte of dilute sulphuric acid
(H 2SO4). This is shown diagrammatically in Fig. 19. The chemical
changes that take place when the cell is discharging and the final
result of the changes are as follows:
(a). At the Positive Plate: Lead peroxide and sulphuric acid produce
lead sulphate, water, and oxygen, or:
[Image] Formula (a). PbO2 + H2SO4 = PbSO4 + H20 + 0
(b). At the Negative Plate: Lead and sulphuric acid produce lead
sulphate and Hydrogen, or:
[Image] Formula (b). Pb + H2SO4 = PbSO4 + H2
[Fig. 20 Chemical Reaction in a Storage Cell during Discharge]
The oxygen of equation (a) and the hydrogen of equation (b) combine to
form water, as may be shown by adding these two equations, giving one
equation for the entire discharge action:
[Image] Formula (c). PbO2 + Pb + 2H2SO4 = 2PbSO4 + 2H2O
In this equation we start with the active materials and electrolyte in
their original condition, and finish with the lead sulphate and water,
which are the final products of a discharge. Examining this equation,
we see that the sulphuric acid of the electrolyte is used up in
forming lead sulphate on both positive and negative plates, and is
therefore removed from the electrolyte. This gives us the easily
remembered rule for remembering discharge actions, which, though open
to question from a strictly scientific viewpoint, is nevertheless
convenient:
During discharge the acid goes into the plates.
The chemical changes described in (a), (b), and (c) are not
instantaneous. That is, the lead, lead peroxide, and sulphuric acid of
the fully charged cell are not changed into lead sulphate and water as
soon as a current begins to pass through the cell. This action is a
gradual one, small portions of these substances being changed at a
time. The greater the current that flows through the cell, the faster
will the changes occur. Theoretically, the changes will continue to
take place as long as any lead, lead peroxide, and sulphuric acid
remain. The faster these are changed into lead sulphate and water, the
shorter will be the time that the storage cell can furnish a current,
or the sooner it will be discharged.
Taking the cell in its discharged condition, let us now connect the
cell to a generator and send current through the cell from the
positive to the negative plates. This is called "charging" the cell.
The lead sulphate and water will now gradually be changed back into
lead, lead peroxide, and sulphuric acid. The lead sulphate which is on
the negative plate is changed to pure lead; the lead sulphate on the
positive plate is changed to lead peroxide, and sulphuric acid will be
added to the water. The changes at the positive plate may be
represented as follows:
Lead sulphate and water produce sulphuric acid, hydrogen and lead
peroxide, or:
[Image] Formula (d). PbSO4 + 2H2O = PbO2 + H2SO4 + H2
The changes at the negative plate may be expressed as follows: Lead
sulphate and water produced sulphuric acid, oxygen, and lead, or:
[Image] Formula (e). PbSO4 + H2o = Pb + H2SO4 + O
The hydrogen (H2) produced at the positive plate, and the oxygen (0)
produced at the negative plate unite to form water, as may be shown by
the equation:
[Image] Formula (f). 2PbSO4 + 2H2O = PbO2 + Pb + 2H2SO4
Equation (f) starts with lead sulphate and water, which, as shown in
equation (c), are produced when a battery is discharged. It will be
observed that we start with lead sulphate and water. Discharged plates
may therefore be charged in water. In fact, badly discharged negatives
may be charged better in water than in electrolyte. The electrolyte is
poured out of the battery and distilled water poured in. The acid
remaining on the separators and plates is sufficient to make the water
conduct the charging current.
In equation (f), the sulphate on the plates combines with water to
form sulphuric acid. This gives us the rule:
During charge, acid is driven out of the plates.
This rule is a convenient one, but, of course, is not a strictly
correct statement.
The changes produced by sending a current through the cell are also
gradual, and will take place faster as the current is made greater.
When all the lead sulphate has been used up by the chemical changes
caused by the current, no further charging can take place. If we
continue to send a current through the cell after it is fully charged,
the water will continue to be split up into hydrogen and oxygen.
Since, however, there is no more lead sulphate left with which the
hydrogen and oxygen can combine to form lead, lead peroxide, and
sulphuric acid, the hydrogen and oxygen rise to the surface of the
electrolyte and escape from the cell. This is known as "gassing", and
is an indication that the cell is fully charged.
Relations Between Chemical Actions and Electricity.
We know now that chemical actions in the battery produce electricity
and that, on the other hand, an electric current, sent through the
battery from an outside source, such as a generator, produces chemical
changes in the battery. How are chemical changes and electricity
related? The various chemical elements which we have in a battery are
supposed to carry small charges of electricity, which, however,
ordinarily neutralize one another. When a cell is discharging,
however, the electrolyte, water, and active materials are separated
into parts carrying negative and positive charges, and these "charges"
cause what we call an electric current to flow in the apparatus
attached to the battery.
Similarly, when a battery is charged, the charging current produces
electrical "charges" which cause the substances in the battery to
unite, due to the attraction of position and negative charges for one
another. This is a brief, rough statement of the relations between
chemical reactions and electricity in a battery. A more thorough study
of the subject would be out of place in this book. It is sufficient
for the repairman to remember that the substances in a battery carry
charges of electricity which become available as an electric current
when a battery discharges, and that a charging current causes electric
charges to form, thereby "charging" the battery.
========================================================================
CHAPTER 5.
WHAT TAKES PLACE DURING DISCHARGE.
----------------------------------
Considered chemically, the discharge of a storage battery consists of
the changing of the spongy lead and lead peroxide into lead sulphate,
and the abstraction of the acid from the electrolyte. Considered
electrically, the changes are more complex, and require further
investigation. The voltage, internal resistance, rate of discharge,
capacity, and other features must be considered, and the effects of
changes in one upon the others must be studied. This proceeding is
simplified considerably if we consider each point separately. The
abstraction of the acid from the electrolyte gives us a method of
determining the condition of charge or discharge in the battery, and
must also be studied.
[Fig. 21 Graph: voltage changes at end and after charge]
Voltage Changes During Discharge. At the end of a charge, and before
opening the charging circuit, the voltage of each cell is about 2.5 to
2.7 volts. As soon as the charging circuit is opened, the cell voltage
drops rapidly to about 2.1 volts, within three or four minutes. This
is due to the formation of a thin layer of lead sulphate on the
surface of the negative plate and between the lead peroxide and the
metal of the positive plate. Fig. 21 shows how the voltage changes
during the last eight minutes of charge, and how it drops rapidly as
soon as the charging circuit is opened. The final value of the voltage
after the charging circuit is opened is about 2.15-2.18 volts. This is
more fully explained in Chapter 6. If a current is drawn from the
battery at the instant the charge is stopped, this drop is more rapid.
At the beginning of the discharge the voltage has already had a rapid
drop from the final voltage on charge, due to the formation of
sulphate as explained above. When a current is being drawn from the
battery, the sudden drop is due to the internal resistance of the
cell, the formation of more sulphate, and the abstracting of the acid
from the electrolyte which fills the pores of the plate. The density
of this acid is high just before the discharge is begun. It is diluted
rapidly at first, but a balanced condition is reached between the
density of the acid in the plates and in the main body of the
electrolyte, the acid supply in the plates being maintained at a
lowered density by fresh acid flowing into them from the main body of
electrolyte. After the initial drop, the voltage decreases more
slowly, the rate of decrease depending on the amount of current drawn
from the battery. The entire process is shown in Fig. 22.
[Fig. 22 Graph: voltage changes during discharge]
Lead sulphate is being formed on the surfaces, and in the body of the
plates. This sulphate has a higher resistance than the lead or lead
peroxide, and the internal resistance of the cell rises, and
contributes to the drop in voltage. As this sulphate forms in the body
of the plates, the acid is used up. At first this acid is easily
replaced from the main body of the electrolyte by diffusion. The acid
in the main body of the electrolyte is at first comparatively strong,
or concentrated, causing a fresh supply of acid to flow into the
plates as fast as it is used up in the plates. This results in the
acid in the electrolyte growing weaker, and this, in turn, leads to a
constant decrease in the rate at which the fresh acid flows, or
diffuses into the plates. Furthermore, the sulphate, which is more
bulky than the lead or lead peroxide fills the pores in the plate,
making it more and more difficult for acid to reach the interior of
the plate. This increases the rate at which the voltage drops.
The sulphate has another effect. It forms a cover over the active
material which has not been acted upon, and makes it practically
useless, since the acid is almost unable to penetrate the coating of
sulphate. We thus have quantities of active material which are
entirely enclosed in sulphate, thereby cutting down the amount of
energy which can be taken from the battery. Thus the formation of
sulphate throughout each plate and the abstraction of acid from the
electrolyte cause the voltage to drop at a constantly increasing rate.
Theoretically, the discharge may be continued until the voltage drops
to zero, but practically, the discharge should be stopped when the
voltage of each cell has dropped to 1.7 (on low discharge rates). If
the discharge is carried on beyond this point much of the spongy lead
and lead peroxide have either been changed into lead sulphate, or have
been covered up by the sulphate so effectively that they are almost
useless. Plates in this condition require a very long charge in order
to remove all the sulphate.
The limiting value of 1.7 volts per cell applies to a continuous
discharge at a moderate rate. At a very high current flowing for only
a very short time, it is not only safe, but advisable to allow a
battery to discharge to a lower voltage, the increased drop being due
to the rapid dilution of the acid in the plates.
The cell voltage will rise somewhat every time the discharge is
stopped. This is due to the diffusion of the acid from the main body
of electrolyte into the plates, resulting in an increased
concentration in the plates. If the discharge has been continuous,
especially if at a high rate, this rise in voltage will bring the cell
up to its normal voltage very quickly on account of the more rapid
diffusion of acid which will then take place.
The voltage does not depend upon the area of the plate surface but
upon the nature of the active materials and the electrolyte. Hence,
although the plates of a cell are gradually being covered with
sulphate, the voltage, measured when no current is flowing, will fall
slowly and not in proportion to the amount of energy taken out of the
cell. It is not until the plates are pretty thoroughly covered with
sulphate, thus making it difficult for the acid to reach the active
material, that the voltage begins to drop rapidly. This is shown
clearly in Fig. 22, which shows that the cell voltage has dropped only
a very small amount when the cell is 50% discharged. With current
flowing through the cell, however, the increased internal resistance
causes a marked drop in the voltage. Open circuit voltage is not
useful, therefore to determine how much energy has been taken from the
battery.
Acid Density. The electrolyte of a lead storage battery is a mixture of
chemically pure sulphuric acid, and chemically pure water, the acid
forming about 30 per cent of the volume of electrolyte when the
battery is fully charged. The pure acid has a "specific gravity" of
1.835, that is, it is 1.835 times as heavy as an equal volume of
water. The mixture of acid and water has a specific gravity of about
1.300. As the cell discharges, acid is abstracted from the
electrolyte, and the weight of the latter must therefore grow less,
since there will be less acid in it. The change in the weight, or
specific gravity of the electrolyte is the best means of determining
the state of discharge of a cell, provided that the cell has been used
properly. In order that the value of the specific gravity may be used
as an indication of the amount of energy in a battery, the history of
the battery must be known. Suppose, for instance, that in refilling
the battery to replace the water lost by the natural evaporation which
occurs in the use of a battery, acid, or a mixture of acid and water
has been used. This will result in the specific gravity being too
high, and the amount of energy in the battery will be less than that
indicated by the specific gravity. Again, if pure water is used to
replace electrolyte which has been spilled, the specific gravity will
be lower than it should be. In a battery which has been discharged to
such an extent that much of the active material has been covered by a
layer of tough sulphate, or if a considerable amount of sulphate and
active material has been loosened from the plates and has dropped to
the bottom of the cells, it will be impossible to bring the specific
gravity of the electrolyte up to 1.300, even though a long charge is
given. There must, therefore, be a reasonable degree of certainty
that a battery has been properly handled if the specific gravity
readings are to be taken as a true indication of the condition of a
battery. Where a battery does not give satisfactory service even
though the specific gravity readings are satisfactory, the latter are
not reliable as indicating the amount of charge in the battery.
As long as a discharge current is flowing from the battery, the acid
within the plates is used up and becomes very much diluted. Diffusion
between the surrounding electrolyte and the acid in the plates keeps
up the supply needed in the plates in order to, carry on the chemical
changes. When the discharge is first begun, the diffusion of acid into
the plates takes place rapidly because there is little sulphate
clogging the pores in the active material, and because there is a
greater difference between the concentration of acid in the
electrolyte and in the plates than will exist as the discharge
progresses. As the sulphate begins to form and fill up the pores of
the plates, and as more and more acid is abstracted from the
electrolyte, diffusion takes place more slowly.
If a battery is allowed to stand idle for a short time after a partial
discharge, the specific gravity of the electrolyte will decrease
because some, of the acid in the electrolyte will gradually flow into
the pores of the plates to replace the acid used up while the battery
was discharging. Theoretically the discharge can be continued until
all the acid has been used up, and the electrolyte is composed of pure
water. Experience has shown, however, that the discharge of the
battery should not be continued after the specific gravity of the
electrolyte has fallen to 1.150. As far as the electrolyte is
concerned, the discharge may be carried farther with safety. The
plates determine the point at which the discharge should be stopped.
When the specific gravity has dropped from 1.300 to 1.150, so much
sulphate has been formed that it fills the pores in the active
material on the plates. Fig. 23 shows the change in the density of the
acid during discharge.
[Fig. 23: Variation of Capacity with Specific Gravity]
Changes at the Negative Plate. Chemically, the action at the negative
plate consists only of the formation of lead sulphate from the spongy
lead. The lead sulphate is only slightly soluble in the electrolyte
and is precipitated as soon as it is formed, leaving hydrogen ions,
which then go to the lead peroxide plate to form water with oxygen
ions released at the peroxide plate. The sulphate forms more quickly
on the surface of the plate than in the inner portions because there
is a constant supply of acid available at the surface, whereas the
formation of sulphate in the interior of the plate requires that acid
diffuse into the pores of the active materials to replace that already
used up in the formation of sulphate. In the negative plate, however,
the sulphate tends to form more uniformly throughout the mass of the
lead, because the spongy lead is more porous than the lead peroxide,
and because the acid is not diluted by the formation of water as in
the positive plate.
Changes at the Positive Plate. In a fully charged positive plate we
have lead peroxide as the active material. This is composed of lead
and oxygen. From this fact it is plainly evident that during discharge
there is a greater chemical activity at this plate than at the
negative plate, since we must find something to combine with the
oxygen in order that the lead may form lead sulphate with the acid.
In an ideal cell, therefore, the material which undergoes the greater
change should be more porous than the material which does not involve
as great a chemical reaction. In reality, however, the peroxide is not
as porous as the spongy lead, and does not hold together as well.
The final products of the discharge of a positive plate are lead
sulphate and water. The lead peroxide must first be reduced to lead,
which then combines with the sulphate from the acid to form lead
sulphate, while the oxygen from the peroxide combines with the
hydrogen of the acid to form water. There is, therefore, a greater
activity at this plate than at the lead plate, and the formation of
the water dilutes the acid in and around the plate so that the
tendency is for the chemical actions to be retarded.
The sulphate which forms on discharge causes the active material to
bulge out because it occupies more space than the peroxide. This
causes the lead peroxide at the surface to begin falling, to the
bottom of the jar in fine dust-like particles, since the peroxide here
holds together very poorly.
========================================================================
CHAPTER 6.
WHAT TAKES PLACE DURING CHARGE.
-------------------------------
Voltage. Starting with a battery which has been discharged until its
voltage has decreased to 1.7 per cell, we pass a current through it
and cause the voltage to rise steadily. Fig. 24 shows the changes in
voltage during charge. Ordinarily the voltage begins to rise
immediately and uniformly. If, however, the battery has been left in a
discharged condition for some time, or has been "over discharged," the
voltage rises very rapidly for a fraction of the first minute of
charge and then drops rapidly to the normal value and thereafter
begins to rise steadily to the end of the charge. This rise at the
beginning of the charge is due to the fact that the density of the
acid in the pores of the plates rises rapidly at first, the acid thus
formed being prevented from diffusing into the surrounding electrolyte
by the coating of sulphate. As soon as this sulphate is broken
through, diffusion takes place and the voltage drops.
[Fig. 24 Graph: voltage changes during charge]
As shown in Fig. 24, the voltage remains almost constant between the
points M and N. At N the voltage begins to rise because the charging
chemical reactions are taking place farther and farther in the inside
parts of the plate, and the concentrated acid formed by the chemical
actions in the plates is diffusing into the main electrolyte. This
increases the battery voltage and requires a higher charging voltage.
At the point marked 0, the voltage begins to rise very rapidly. This
is due to the fact that the amount of lead sulphate in the plates is
decreasing very rapidly, allowing the battery voltage to rise and thus
increasing the charging voltage. Bubbles of gas are now rising through
the electrolyte.
At P, the last portions of lead sulphate are removed, acid is no
longer being formed, and hydrogen and oxygen gas are formed rapidly.
The gas forces the last of the concentrated acid out of the plates and
in fact, equalizes the acid concentration throughout the whole cell.
Thus no further changes can take place, and the voltage becomes
constant at R at a voltage of 2.5 to 2.7.
Density of Electrolyte. Discharge should be stopped when the density
of the electrolyte, as measured with a hydrometer, is 1.150. When we
pass a charging current through the battery, acid is produced by the
chemical actions which take place in the plates. This gradually
diffuses with the main electrolyte and causes the hydrometer to show a
higher density than before. This increase in density continues
steadily until the battery begins to "gas" freely.
The progress of the charge is generally determined by the density of
the electrolyte. For this purpose in automobile batteries, a
hydrometer is placed in a glass syringe having a short length of
rubber tubing at one end, and a large rubber bulb at the other. The
rubber tube is inserted in the cell and enough electrolyte drawn up
into the syringe to float the hydrometer so as to be able to obtain a
reading. This subject will be treated more fully in a later chapter.
Changes at Negative Plate. The charging current changes lead sulphate
into spongy lead, and acid is formed. The acid is mixed with the
diluted electrolyte outside of the plates. As the charging proceeds
the active material shrinks or contracts, and the weight of the plate
actually decreases on account of the difference between the weight and
volume of the lead sulphate and spongy lead. If the cell has had only
a normal discharge and the charge is begun soon after the discharge
ended, the charge will proceed quickly and without an excessive rise
in temperature. If, however, the cell has been discharged too far, or
has been in a discharged condition for some time, the lead sulphate
will not be in a finely divided state as it should be, but will be
hard and tough and will have formed an insulating coating over the
active material, causing the charging voltage to be high, and the
charge will proceed slowly. When most of the lead sulphate has been
reduced to spongy lead, the charging current will be greater than is
needed to carry on the chemical actions, and will simply decompose the
water into hydrogen and oxygen, and the cell "gasses." Spongy lead is
rather tough and coherent, it, and the bubbles of gas which form in
the pores of the negative plate near the end of the charge force their
way to the surface without dislodging any of the active material.
Changes at the Positive Plate. When a cell has been discharged, a
portion of the lead peroxide has been changed to lead sulphate, which
has lodged in the pores of the active material and on its surface.
During charge, the lead combines with oxygen from the water to form
lead peroxide, and acid is formed. This acid diffuses into the
electrolyte as fast as the amount of sulphate will permit. If the
discharge has been carried so far that a considerable amount of
sulphate has formed in the pores and on the surface of the plate, the
action proceeds very slowly, and unless a moderate charging current is
used, gassing begins before the charge is complete, simply because the
sulphate cannot absorb the current. The gas bubbles which originate in
the interior of the plate force their way to the surface, and in so
doing cause numerous fine particles of active material to break off
and fall to the bottom of the jar. This happens because the lead
peroxide is a granular, non-coherent substance, with the particles
held together very loosely, and the gas breaks off a considerable
amount of active material.
========================================================================
CHAPTER 7.
CAPACITY OF STORAGE BATTERIES.
------------------------------
The capacity of a storage battery is the product of the current drawn
from a battery, multiplied by the number of hours this current flows.
The unit in which capacity is measured is the ampere-hour.
Theoretically, a battery has a capacity of 40 ampere hours if it
furnishes ten amperes for four hours, and if it is unable, at the end
of that time, to furnish any more current. If we drew only five
amperes from this battery, it should be able to furnish this current
for eight hours. Thus, theoretically, the capacity of a battery should
be the same, no matter what current is taken from it. That is, the
current in amperes, multiplied by the number of hours the battery,
furnished this current should be constant.
In practice, however, we do not discharge a battery to a lower voltage
than 1.7 per cell, except when the rate of discharge is high, such as
is the case when using the starting motor, on account of the
increasing amount of sulphate and the difficulty with which this is
subsequently removed and changed into lead and lead peroxide. The
capacity of a storage battery is therefore measured by the number of
ampere hours it can furnish before its voltage drops below 1.7 per
cell. This definition assumes that the discharge is a continuous one,
that we start with a fully charged battery and discharge it
continuously until its voltage drops to 1.7 per cell.
The factors upon which the capacity of storage batteries depend may be
grouped in two main classifications:
1. Design and Construction of Battery
2. Conditions of Operation
Design and Construction.
Each classification may be subdivided. Under the Design and
Construction we have:
(a) Area of plate surface.
(b) Quantity, arrangement, and porosity of active materials.
(c) Quantity and strength of electrolyte.
(d) Circulation of electrolyte.
These sub-classifications require further explanation. Taking them in
order:
(a) Area of Plate Surface. It is evident that the chemical and
electrical activity of a battery are greatest at the surface of the
plates since the acid and active material are in intimate contact
here, and a supply of fresh acid is more readily available to replace
that which is depleted as the battery is discharged. This is
especially true with high rates of discharge, such as are caused in
starting automobile engines. Therefore, the capacity of a battery will
be greater if the surface area of its plates is increased. With large
plate areas a greater amount of acid and active materials is
available, and an increase in capacity results.
(b) Quantity, Arrangement, and Porosity of Active Materials. Since the
lead and lead peroxide are changed to lead sulphate on discharge, it
is evident that the greater the amount of these materials, the longer
can the discharge continue, and hence the greater the capacity.
The arrangement of the active materials is also important, since the
acid and active materials must be in contact in order to produce
electricity. Consequently the capacity will be greater in a battery,
all of whose active materials are in contact with the acid, than in
one in which the acid reaches only a portion of the active materials.
It is also important that all parts of the plates carry the same
amount of current, in order that the active materials may be used
evenly. As a result of these considerations, we find that the active
materials are supported on grids of lead, that the plates are made
thin, and that they have large surface areas. For heavy discharge
currents, such as starting motor currents, it is essential that there
be large surface areas. Thick plates with smaller surface areas are
more suitable for low discharge rates.
Since the inner portions of the active materials must have a plentiful
and an easily renewable supply of acid, the active materials must be
porous in order that diffusion may be easy and rapid.
(c) Quantity and Strength of Electrolyte. It is important that there
be enough electrolyte in order that the acid may not become exhausted
while there is still considerable active material left. An
insufficient supply of electrolyte makes it impossible to obtain the
full capacity from a battery. On the other hand, too much electrolyte,
due either to filling the battery too full, or to having the plates in
a jar that holds too much electrolyte, results in an increase in
capacity up to the limit of the plate capacity. There is a danger
present, however, because with an excess of electrolyte the plates
will be discharged before the specific gravity of the electrolyte
falls to 1.150. This results in over discharge of the battery with its
attendant troubles as will be described more fully in a later chapter.
It is a universal custom to consider a battery discharged when the
specific gravity of the electrolyte has dropped to 1.150, and that it
is fully charged when the specific gravity of the electrolyte has
risen to 1.280-1.300. This is true in temperate climates. In tropical
countries, which may for this purpose be defined as those countries in
which the temperature never falls below the freezing point, the
gravity of a fully charged cell is 1.200 to 1.230. The condition of
the plates is, however, the true indicator of charged or discharged
condition. With the correct amount of electrolyte, its specific
gravity is 1.150 when the plates have been discharged as far as it is
considered safe, and is 1.280-1.300 when the plates are fully charged.
When electrolyte is therefore poured into a battery, it is essential
that it contains the proper proportion of acid and water in order that
its specific gravity readings be a true indicator of the condition of
the plates as to charge or discharge, and hence show accurately how
much energy remains in the cell at any time.
A question which may be considered at this point is why in automobile,
work a specific gravity of 1.280-1.300 is adopted for the electrolyte
of a fully charged cell. There are several reasons. The voltage of a
battery increases as the specific gravity goes up. Hence, with a
higher density, a higher voltage can be obtained. If the density were
increased beyond this point, the acid would attack the lead grids and
the separators, and considerable corrosion would result. Another
danger of high density is that of sulphation, as explained in a later
chapter. Another factor which enters is the resistance of the
electrolyte. It is desirable that this be as low as possible. If we
should make resistance measurements on various mixtures of acid and
water, we should find that with a small percentage of acid, the
resistance is high. As the amount of acid is increased, the resistance
will grow less up to a certain point. Beyond this point, the
resistance will increase again as more acid is added to the mixture.
The resistance is lowest when the acid forms 30% of the electrolyte.
Thus, if the electrolyte is made too strong, the plates and also the
separators will be attacked by the acid, and the resistance of the
electrolyte will also increase. The voltage increases as the
proportion of acid is increased, but the other factors limit the
concentration. If the electrolyte is diluted, its resistance rises,
and the amount of acid is insufficient to give much capacity. The
density of 1.280-1.300 is therefore a compromise between the various
factors mentioned above.
(d) Circulation of Electrolyte. This refers to the passing of
electrolyte from one plate to another, and depends upon the ease with
which the acid can pass through the pores of the separators. A porous
separator allows more energy to be drawn from the battery than a
nonporous one.
Operating Conditions.
Considering now the operating conditions, we find several items to be
taken into account. The most important are:
(e) Rate of discharge.
(f) Temperature.
(e) Rate of Discharge. As mentioned above, the ampere hour rating of a
battery is based upon a continuous discharge, starting with a specific
gravity of 1.280-1.300, and finishing with 1.150. The end of the
discharge is also considered to be reached when the voltage per cell
has dropped to 1.7. With moderate rates of discharge the acid is
abstracted slowly enough to permit the acid from outside the plates to
diffuse into the pores of the plates and keep up the supply needed for
the chemical actions. With increased rates of discharge the supply of
acid is used up so rapidly that the diffusion is not fast enough to
hold up the voltage. This fact is shown clearly by tests made to
determine the time required to discharge a 100 Amp. Hr., 6 volt
battery to 4.5 volts. With a discharge rate of 25 amperes, it required
160 minutes. With a discharge rate of 75 amperes, it required 34
minutes. From this we see that making the discharge rate three times
as great caused the battery to be discharged in one fifth the time.
These discharges were continuous, however, and if the battery were
allowed to rest, the voltage would soon rise sufficiently, to burn the
lamps for a number of hours.
The conditions of operation in automobile work are usually considered
severe. In starting the engine, a heavy current is drawn from the
battery for a few seconds. The generator starts charging the battery
immediately afterward, and the starting energy is soon replaced. As
long as the engine runs, there is no load on the battery, as the
generator will furnish the current for the lamps, and also send a
charge into the battery. If the lamps are not used, the entire
generator output is utilized to charge the battery, unless some
current is furnished to the ignition system. Overcharge is quite
possible.
When the engine is not running, the lamps are the only load on the
battery, and there is no charging current. Various drivers have
various driving conditions. Some use their starters frequently, and
make only short runs. Their batteries run down. Other men use the
starter very seldom, and take long tours. Their batteries will be
overcharged. The best thing that can be done is to set the generator
for an output that will keep the battery charged under average
conditions.
From the results of actual tests, it may be said that modem lead-acid
batteries are not injured in any way by the high discharge rate used
when a starting motor cranks the engine. It is the rapidity with which
fresh acid takes the place of that used in the pores of the active
materials that affects the capacity of a battery at high rates, and
not only limitation in the plates themselves. Low rates of discharge
should, in fact, be avoided more than the high rates. Battery capacity
is affected by discharge rates, only when the discharge is continuous,
and the reduction in capacity caused by the high rates of continuous
discharge does not occur if the discharge is an intermittent one, such
as is actually the case in automobile work. The tendency now is to
design batteries to give their rated capacity in very short discharge
periods. If conditions should demand it, these batteries would be sold
to give their rated capacity while operating intermittently at a rate
which would completely discharge them in three or four minutes. The
only change necessary for such high rates of discharge is to provide
extra heavy terminals to carry the heavy current.
The present standard method of rating starting and lighting batteries,
as recommended by the Society of Automotive Engineers, is as follows:
"Batteries for combined lighting and starting service shall have two
ratings. The first shall indicate the lighting ability, and shall be
the capacity in ampere hours of the battery when discharged
continuously at the 5 hour rate to a final voltage of not less than
1.7 per cell, the temperature of the battery beginning such discharge
being 80°F. The second rating shall indicate the starting ability and
shall be the capacity in ampere-hours when the battery is discharged
continuously at the 20-minute rate to a final voltage of not less than
1.5 per cell, the temperature of the battery beginning such discharge
being 80°F."
The discharge rate required under the average starting conditions is
higher than that specified above, and would cause the required drop in
voltage in about fifteen minutes. In winter, when an engine is cold
and stiff, the work required from the battery is even more severe, the
discharge rate being equivalent in amperes to probably four or five
times the ampere-rating of the battery. On account of the rapid
recovery of a battery after a discharge at a very high rate, it seems
advisable to allow a battery to discharge to a voltage of 1.0 per cell
when cranking an engine which is extremely cold and stiff.
(f) Temperature. Chemical reactions take place much more readily at
high temperatures than at low. Furthermore, the active materials are
more porous, the electrolyte lighter, and the internal resistance less
at higher temperatures. Opposed to this is the fact that at high
temperatures, the acid attacks the grids and active materials, and
lead sulphate is formed, even though no current is taken from the
battery. Other injurious effects are the destructive actions of hot
acid on the wooden separators used in most starting and lighting
batteries. Greater expansion of active material will also occur, and
this expansion is not, in general, uniform over the surface of the
plates. This results in unequal strains and the plates are bent out of
shape, or "buckled." The expansion of the active material will also
cause much of it to fall from the plates, and we then have "shedding."
[Fig. 25 Graph: Theoretical temperature changes during charge
and discharge]
When sulphuric acid is poured into water, a marked temperature rise
takes place. When a battery is charged, acid is formed, and when this
mixes with the diluted electrolyte, a temperature rise occurs. In
discharging, acid is taken from the electrolyte, and the temperature
has a tendency to drop. On charging, therefore, there is danger of
overheating, while on discharge, excessive temperatures are not
likely. Fig. 25 shows the theoretical temperature changes on charge
and discharge. The decrease in temperature given-in the curve is not
actually obtained in practice, because the tendency of the temperature
to decrease is balanced by the heat caused by the current passing
through the battery.
Age of Battery.
Another factor which should be considered in connection with capacity
is the age of the battery. New batteries often do not give their rated
capacity when received from the manufacturer. This is due to the
methods of making the plates. The "paste" plates, such as are used in
automobiles, are made by applying oxides of lead, mixed with a liquid,
which generally is dilute sulphuric acid, to the grids. These oxides
must be subjected to a charging current in order to produce the spongy
lead and lead peroxide. After the charge, they must be discharged, and
then again charged. This is necessary because not all of the oxides
are changed to active material on one charge, and repeated charges and
discharges are required to produce the maximum amount of active
materials. Some manufacturers do not charge and discharge a battery a
sufficient number of times before sending it out, and after a battery
is put into use, its capacity will increase for some time, because
more active material is produced during each charge.
Another factor which increases the capacity of a battery after it is
put into use is the tendency of the positive active material to become
more porous after the battery is put through the cycles of charge and
discharge. This results in an increase in capacity for a considerable
time after the battery is put into use.
When, a battery has been in use for some time, a considerable portion
of the active material will have fallen from the positive plates, and,
a decrease in capacity will result. Such a battery will charge faster
than a new one because the amount of sulphate which has formed when
the battery is discharged is less than in a newer battery. Hence, the
time required to reduce this sulphate will be less, and the battery
will "come up" faster on charge, although the specific gravity of the
electrolyte may not rise to 1.280.
========================================================================
CHAPTER 8.
INTERNAL RESISTANCE.
--------------------
The resistance offered by a storage battery to the flow of a current
through it results in a loss of voltage, and in heating. Its value
should be as low as possible, and, in fact, it is almost negligible
even I in small batteries, seldom rising above 0.05 ohm. On charge, it
causes the charging voltage to be higher and on discharge causes a
loss of voltage. Fig. 26 shows the variation in resistance.
[Fig. 26 Graph: Changes in internal resistance during charge
and discharge]
The resistance as measured between the terminals of a cell is made up
of several factors as follows:
1. Grids. This includes the resistance of the terminals, connecting
links, and the framework upon which the active materials are pasted.
This is but a small part of the total resistance, and does not
undergo any considerable change during charge and discharge. It
increases slightly as the temperature of the grids rises.
2. Electrolyte. This refers to the electrolyte between the plates, and
varies with the amount of acid and with temperature. As mentioned in
the preceding chapter, a mixture of acid and water in which the acid
composes thirty per cent of the electrolyte has the minimum
resistance. Diluting or increasing the concentration of the
electrolyte will both cause an increase in resistance from the minimum
I value. The explanation probably lies in the degree to which the acid
is split up into "ions" of hydrogen (H), and sulphate (SO4). These
"ions" carry the current through t he electrolyte. Starting with a
certain amount of acid, let us see how the ionization progresses. With
very concentrated acid, ionization does not take place, and hence,
there are no ions to carry current. As we mix the acid with water,
ionization occurs. The more water used, the more ions, and hence, the
less the resistance, because the number of ions available to carry the
current increases. The ionization in creases to a certain maximum
degree, beyond which no more ions are formed. It is probable that an
electrolyte containing thirty per cent of acid is at its maximum
degree of ionization and hence its lowest resistance. If more water is
now added, no more ions are formed. Furthermore, the number of ions
per unit volume of electrolyte will now decrease on account of the
increased amount of water. There Will therefore be fewer ions per unit
volume to carry the current, and the resistance of the electrolyte
increases.
With an electrolyte of a given concentration, an increase of
temperature will cause a decrease in resistance. A decrease in
temperature will, of course, cause an increase in resistance. It is
true, in general, that the resistance of the electrolyte is about half
of the total resistance of the cell. The losses due to this resistance
generally form only one per cent of the total losses, and area
practically negligible factor.
3. Active Material. This includes the resistance of the active
Cite this
Otto A. Witte. "The Automobile Storage Battery: Its Care And Repair". Project Gutenberg. Public domain in the USA. https://www.gutenberg.org/ebooks/29718